Specific Process Knowledge/Lithography/ZEP520A: Difference between revisions
Appearance
No edit summary |
|||
| (15 intermediate revisions by 3 users not shown) | |||
| Line 1: | Line 1: | ||
This is a standard positive resist from ZEON. The resist is very expensive; DTU Nanolab has thus stopped buying this resist. | |||
Use CSAR instead. | |||
== Spin Curves == | == Spin Curves == | ||
| Line 115: | Line 10: | ||
The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on a Si wafer with native oxide. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus | The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on a Si wafer with native oxide. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus represents the homogeinity of the film on the 4" wafers. | ||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 40%" | {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 40%" | ||
| Line 122: | Line 17: | ||
|- | |- | ||
|-style="background:Black; color:White" | |-style="background:Black; color:White" | ||
!colspan="7"|ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 23-04-2014. Resist was mixed 13-01-2014, i.e. | !colspan="7"|ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 23-04-2014. Resist was mixed 13-01-2014, i.e. approximately 3 months old. | ||
|- | |- | ||
| Line 167: | Line 62: | ||
|- | |- | ||
|-style="background:red; color:White" | |-style="background:red; color:White" | ||
!colspan="7"|ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. | !colspan="7"|ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximately 6 days old. | ||
|- | |- | ||
| Line 227: | Line 122: | ||
|- | |- | ||
|-style="background:green; color:White" | |-style="background:green; color:White" | ||
!colspan="7"|ZEON ZEP520A1:2 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. | !colspan="7"|ZEON ZEP520A1:2 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximately 6 days old. | ||
|- | |- | ||
Latest revision as of 21:57, 25 August 2025
This is a standard positive resist from ZEON. The resist is very expensive; DTU Nanolab has thus stopped buying this resist.
Use CSAR instead.
Spin Curves

The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on a Si wafer with native oxide. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus represents the homogeinity of the film on the 4" wafers.
| ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 23-04-2014. Resist was mixed 13-01-2014, i.e. approximately 3 months old. | ||||||
|---|---|---|---|---|---|---|
| Spin Speed [rpm] | Acceleration [1/s2] | Thickness [nm] | St Dev | |||
| 3000 | 4000 | 111.29 | 0.65 | |||
| 4000 | 4000 | 95.17 | 2.16 | |||
| 5000 | 4000 | 87.23 | 0.81 | |||
| ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximately 6 days old. | ||||||
|---|---|---|---|---|---|---|
| Spin Speed [rpm] | Acceleration [1/s2] | Thickness [nm] | St Dev | |||
| 2000 | 4000 | 141.03 | 1.02 | |||
| 3000 | 4000 | 115.96 | 0.98 | |||
| 4000 | 4000 | 100.56 | 0.80 | |||
| 5000 | 4000 | 91.01 | 0.38 | |||
| 6000 | 4000 | 84.85 | 0.37 | |||
| ZEON ZEP520A1:2 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximately 6 days old. | ||||||
|---|---|---|---|---|---|---|
| Spin Speed [rpm] | Acceleration [1/s2] | Thickness [nm] | St Dev | |||
| 2000 | 4000 | 79.12 | 1.74 | |||
| 3000 | 4000 | 64.30 | 0.34 | |||
| 4000 | 4000 | 55.50 | 0.48 | |||
| 5000 | 4000 | 50.53 | 0.62 | |||
| 6000 | 4000 | 46.34 | 1.01 | |||