Specific Process Knowledge/Lithography/ZEP520A: Difference between revisions
Appearance
No edit summary |
|||
| (36 intermediate revisions by 3 users not shown) | |||
| Line 1: | Line 1: | ||
This is a standard positive resist from ZEON. The resist is very expensive; DTU Nanolab has thus stopped buying this resist. | |||
Use CSAR instead. | |||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | == Spin Curves == | ||
[[File:SpinCurveZEP520A.png|right|700px]] | |||
The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on a Si wafer with native oxide. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus represents the homogeinity of the film on the 4" wafers. | |||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 40%" | |||
|- | |- | ||
|- | |- | ||
|-style="background:Black; color:White" | |-style="background:Black; color:White" | ||
! | !colspan="7"|ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 23-04-2014. Resist was mixed 13-01-2014, i.e. approximately 3 months old. | ||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:silver; color:black" style="text-align:left;" | ||
! | !Spin Speed [rpm] | ||
!Acceleration [1/s2] | |||
!Thickness [nm] | |||
!St Dev | |||
|- | |- | ||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|3000 | |||
|4000 | |||
|111.29 | |||
|0.65 | |||
|- | |||
|- | |- | ||
|-style="background: | |-style="background:WhiteSmoke; color:black" | ||
| | |4000 | ||
| | |4000 | ||
| | |95.17 | ||
| | |2.16 | ||
|- | |- | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black | |-style="background:WhiteSmoke; color:black" | ||
|5000 | |||
|4000 | |||
|87.23 | |||
|0.81 | |||
|- | |- | ||
| | |} | ||
| | {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 40%" | ||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:red; color:White" | ||
| | !colspan="7"|ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximately 6 days old. | ||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:silver; color:black" style="text-align:left;" | ||
! | !Spin Speed [rpm] | ||
!Acceleration [1/s2] | |||
!Thickness [nm] | |||
!St Dev | |||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:WhiteSmoke; color:black" | ||
| | |2000 | ||
| | |4000 | ||
|141.03 | |||
| | |1.02 | ||
| | |||
|- | |- | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black | |-style="background:WhiteSmoke; color:black" | ||
|3000 | |||
|4000 | |||
|115.96 | |||
|0.98 | |||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:WhiteSmoke; color:black" | ||
| | |4000 | ||
| | |4000 | ||
|100.56 | |||
|0.80 | |||
| | |||
| | |||
|- | |- | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black | |-style="background:WhiteSmoke; color:black" | ||
|5000 | |||
|4000 | |||
|91.01 | |||
|0.38 | |||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:WhiteSmoke; color:black" | ||
| | |6000 | ||
| | |4000 | ||
| | |84.85 | ||
| | |0.37 | ||
|- | |- | ||
|} | |} | ||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 40%" | |||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | |||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:green; color:White" | ||
!colspan="7"|ZEON ZEP520A1: | !colspan="7"|ZEON ZEP520A1:2 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximately 6 days old. | ||
|- | |- | ||
|- | |- | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" style="text-align:left;" | ||
!Spin Speed [rpm] | !Spin Speed [rpm] | ||
!Acceleration [1/s2] | !Acceleration [1/s2] | ||
!Thickness [nm] | !Thickness [nm] | ||
!St Dev | !St Dev | ||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|2000 | |||
|4000 | |||
|79.12 | |||
|1.74 | |||
|- | |- | ||
| Line 135: | Line 145: | ||
|3000 | |3000 | ||
|4000 | |4000 | ||
| | |64.30 | ||
|0. | |0.34 | ||
|- | |- | ||
| Line 143: | Line 153: | ||
|4000 | |4000 | ||
|4000 | |4000 | ||
| | |55.50 | ||
| | |0.48 | ||
|- | |- | ||
| Line 151: | Line 161: | ||
|5000 | |5000 | ||
|4000 | |4000 | ||
| | |50.53 | ||
|0. | |0.62 | ||
|- | |- | ||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|6000 | |||
|4000 | |||
|46.34 | |||
|1.01 | |||
|- | |||
|} | |} | ||
Latest revision as of 21:57, 25 August 2025
This is a standard positive resist from ZEON. The resist is very expensive; DTU Nanolab has thus stopped buying this resist.
Use CSAR instead.
Spin Curves

The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on a Si wafer with native oxide. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus represents the homogeinity of the film on the 4" wafers.
| ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 23-04-2014. Resist was mixed 13-01-2014, i.e. approximately 3 months old. | ||||||
|---|---|---|---|---|---|---|
| Spin Speed [rpm] | Acceleration [1/s2] | Thickness [nm] | St Dev | |||
| 3000 | 4000 | 111.29 | 0.65 | |||
| 4000 | 4000 | 95.17 | 2.16 | |||
| 5000 | 4000 | 87.23 | 0.81 | |||
| ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximately 6 days old. | ||||||
|---|---|---|---|---|---|---|
| Spin Speed [rpm] | Acceleration [1/s2] | Thickness [nm] | St Dev | |||
| 2000 | 4000 | 141.03 | 1.02 | |||
| 3000 | 4000 | 115.96 | 0.98 | |||
| 4000 | 4000 | 100.56 | 0.80 | |||
| 5000 | 4000 | 91.01 | 0.38 | |||
| 6000 | 4000 | 84.85 | 0.37 | |||
| ZEON ZEP520A1:2 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximately 6 days old. | ||||||
|---|---|---|---|---|---|---|
| Spin Speed [rpm] | Acceleration [1/s2] | Thickness [nm] | St Dev | |||
| 2000 | 4000 | 79.12 | 1.74 | |||
| 3000 | 4000 | 64.30 | 0.34 | |||
| 4000 | 4000 | 55.50 | 0.48 | |||
| 5000 | 4000 | 50.53 | 0.62 | |||
| 6000 | 4000 | 46.34 | 1.01 | |||