Jump to content

Specific Process Knowledge/Lithography/Coaters/SprayCoater: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
No edit summary
Taran (talk | contribs)
No edit summary
 
(23 intermediate revisions by 6 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:CustomerSupport@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters/SprayCoater click here]'''
{{cc-nanolab}}


'''Feedback to this page''': '''[mailto:CustomerSupport@Nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters/SprayCoater click here]'''


==Spray Coater==
==Spray Coater==
The spray coater at Danchip is located in Cleanroom C-1. The machine is an ExactaCoat from Sono-tek which can be fitted with one of three different nozzles depending on the nature of the spray coating tasks at hand. The three different nozzles (Impact, AccuMist and Vortex) are optimized for different applications such as spray coating of large areas (e.g. entire wafers), smaller areas (e.g. wafer pieces or other small samples) or already structured samples that cannot be coated uniformly by spin coating. All nozzles use an ultrasonic tranducer for atomizing the solution to be spray coated. It is therefore a prerequisite that all components are compatible with this process. This is the case with most substances, although process parameters may need optimization to give satisfactory results.
[[image:1042_spraycoater_overview.jpg|400x239px|right|thumb|Spray Coater is located in Serviceroom Cx1]]


Practically any sample that will fit inside the spray coater can be processed. Spray patterns are easily programmed either using predefined spray patterns (1D line, 2D rectangles/circles/meanders/spirals or custom 3D spray patterns).
The spray coater at DTU Nanolab is located in Cleanroom C-1. The machine is an ExactaCoat from Sono-tek which can be fitted with one of three different nozzles depending on the nature of the spray coating tasks at hand. The three different nozzles (Impact, AccuMist and Vortex) are optimized for different applications such as spray coating of large areas (e.g. entire wafers), smaller areas (e.g. wafer pieces or other small samples) or already structured samples that cannot be coated uniformly by spin coating. All nozzles use an ultrasonic transducer for atomizing the solution to be spray coated. It is therefore a prerequisite that all components are compatible with this process. This is the case with most substances, although process parameters may need optimization to give satisfactory results.


The spray coating process as well as major features of the three nozzles are described into more detail in the manual which can be found via the Equipment Info page in LabManager. It can be found be clicking Equipment -> Info or by using the direct link below. Then follow the 'User Manual' link.
Practically any sample that will fit inside the spray coater can be processed. Spray patterns are easily programmed either using predefined spray patterns (1D line, 2D rectangles/circles/meanders/spirals) or custom 3D spray patterns.


'''The user manual(s), quality control procedure(s) and results, user APV(s), technical information and contact information can be found in [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=293 LabManager]'''
The spray coating process as well as major features of the three nozzles are described into more detail in the manual which can be found via the Equipment Info page in LabManager under the Documents sections. The manual can also be found by clicking [http://labmanager.dtu.dk/d4Show.php?id=2523&mach=293 this direct link].


'''Further information about the spray coater (manual, process log, technical information etc.) can be found in LabManger''':
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=293 Spray coater in LabManager]'''
== Process development==
*[[/AZ4562|Spray coating using AZ4562]]
*[[/TISpray|Spray coating using TI Spray]]
==Equipment performance and process related parameters==


[[image:1042_spraycoater_overview.jpg|400x239px|right|thumb|Spray Coater in Cleanroom C-1]]
{| border="2" cellspacing="0" cellpadding="2"  
{| border="2" cellspacing="0" cellpadding="2"  


Line 21: Line 30:
|style="background:LightGrey; color:black"|  
|style="background:LightGrey; color:black"|  
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Spraying imprint resist
*Spraying imprint resists  (primarily mr-NIL 6000E and mr-I 8000E)
*Spraying photoresist
*Spraying photoresist (primarily AZ-4562)
*Spraying of other solutions
*Spraying of other solutions
|-
|-
Line 28: Line 37:
|style="background:LightGrey; color:black"|Substrate handling
|style="background:LightGrey; color:black"|Substrate handling
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* Can handle almost any sample size and shape
* Can handle almost any sample size and shape (although no automatic handling)
|-
|-
|style="background:LightGrey; color:black"|Permanent media
|style="background:LightGrey; color:black"|Permanent media
Line 41: Line 50:
|style="background:LightGrey; color:black"|Solution viscosity
|style="background:LightGrey; color:black"|Solution viscosity
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Range
*Should not exceed 20 cP
|-
|-
|style="background:LightGrey; color:black"|Chemical properties
|style="background:LightGrey; color:black"|Chemical properties
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Must be non-toxic
*Must be non-toxic
*Compatible with titanium
*Must be compatible with titanium
*Resistant to ultrasonic atomization
*Resistant to ultrasonic sonication
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Batch size
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Any sample(s) that fit inside machine
*Any sample(s) size and number that fit inside machine
|-
|-
| style="background:LightGrey; color:black"|Allowed materials
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*All chemicals to be spray coated must be approved specifically for spray coating
*'''All chemicals to be spray coated must be approved specifically for spray coating'''
*Any non-toxic, non-particulate and non-crosslinking material is likely to be approved
*Most non-toxic, non-particulate and non-crosslinking material likely to be approved
*Suspensions challenging due to very low diameter tubing
|-  
|-  
|}
|}

Latest revision as of 16:10, 25 August 2025

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Spray Coater

Spray Coater is located in Serviceroom Cx1

The spray coater at DTU Nanolab is located in Cleanroom C-1. The machine is an ExactaCoat from Sono-tek which can be fitted with one of three different nozzles depending on the nature of the spray coating tasks at hand. The three different nozzles (Impact, AccuMist and Vortex) are optimized for different applications such as spray coating of large areas (e.g. entire wafers), smaller areas (e.g. wafer pieces or other small samples) or already structured samples that cannot be coated uniformly by spin coating. All nozzles use an ultrasonic transducer for atomizing the solution to be spray coated. It is therefore a prerequisite that all components are compatible with this process. This is the case with most substances, although process parameters may need optimization to give satisfactory results.

Practically any sample that will fit inside the spray coater can be processed. Spray patterns are easily programmed either using predefined spray patterns (1D line, 2D rectangles/circles/meanders/spirals) or custom 3D spray patterns.

The spray coating process as well as major features of the three nozzles are described into more detail in the manual which can be found via the Equipment Info page in LabManager under the Documents sections. The manual can also be found by clicking this direct link.

Further information about the spray coater (manual, process log, technical information etc.) can be found in LabManger:

Spray coater in LabManager

Process development

Equipment performance and process related parameters

Equipment Spray Coater
Purpose
  • Spraying imprint resists (primarily mr-NIL 6000E and mr-I 8000E)
  • Spraying photoresist (primarily AZ-4562)
  • Spraying of other solutions
Performance Substrate handling
  • Can handle almost any sample size and shape (although no automatic handling)
Permanent media
  • No permanent media
Manual dispense option
  • Two syringe pumps
Process parameter range Solution viscosity
  • Should not exceed 20 cP
Chemical properties
  • Must be non-toxic
  • Must be compatible with titanium
  • Resistant to ultrasonic sonication
Substrates Batch size
  • Any sample(s) size and number that fit inside machine
Allowed materials
  • All chemicals to be spray coated must be approved specifically for spray coating
  • Most non-toxic, non-particulate and non-crosslinking material likely to be approved
  • Suspensions challenging due to very low diameter tubing