= Deposition of Niobium =
'''Feedback to this page''': '''[mailto:LabAdviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Niobium click here]'''
 
<i> This page is written by <b>DTU Nanolab staff</b></i>
 
== Deposition of Nb ==
Niobium can be deposited by e-beam evaporation or sputtering. In the chart below you can compare the deposition equipment.
Niobium can be deposited by e-beam evaporation or sputtering. In the chart below you can compare the deposition equipment.


Line 30: Line 25:
!Pre-clean
!Pre-clean
|Ar ion bombardment
|Ar ion bombardment
|RF Ar clean
|none
|RF Ar clean
|RF Ar clean


Line 96: Line 91:
| Substrates get heated during the deposition.  
| Substrates get heated during the deposition.  
For 100 nm Nb at 2 Å/s, the substrate reached about 105 °C.
For 100 nm Nb at 2 Å/s, the substrate reached about 105 °C.
|
|
|
|}
|}

Latest revision as of 14:56, 9 August 2025

Deposition of Niobium

Niobium can be deposited by e-beam evaporation or sputtering. In the chart below you can compare the deposition equipment.

E-beam evaporation (Temescal) Sputter deposition (Lesker) Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3))
General description E-beam deposition of Nb

(line-of-sight deposition)

Sputter deposition of Nb

(not line-of-sight deposition)

Sputter deposition of Nb

(not line-of-sight deposition)

Pre-clean Ar ion bombardment none RF Ar clean
Layer thickness 10Å to 200 nm* 10Å to 600 nm** ask staff, probably similar to old Lesker sputter system
Deposition rate 0.5Å/s to 5Å/s ~1Å/s ? Probably similar to old Lesker sputter system
Batch size
  • Up to 4x6" wafers
  • Up to 3x8" wafers (ask for holder)
  • smaller pieces
  • smaller pieces
  • Up to 1x6" wafers
  • Up to 10x4" or 6" wafers
  • Many smaller pieces
Allowed materials
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Almost any that do not outgas.


Comment Substrates get heated during the deposition.

For 100 nm Nb at 2 Å/s, the substrate reached about 105 °C.

* To deposit layers thicker than 200 nm permission is required to ensure that there is enough metal (contact metal@nanolab.dtu.dk)

** To deposit layers thicker than 600 nm permission is required to ensure that there is enough metal (contact metal@nanolab.dtu.dk)