Specific Process Knowledge/Characterization/SEM Supra 1: Difference between revisions
No edit summary |
|||
| (21 intermediate revisions by 3 users not shown) | |||
| Line 1: | Line 1: | ||
= | '''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Characterization/SEM_Supra_1 click here]''' | ||
<!--Checked for updates on 30/7-2018 - ok/jmli --> | |||
''This page is written by DTU Nanolab internal'' | |||
[[image:LA_SEM_Supra_1.jpg|400x400px|right|thumb|The SEM Supra 1 located in basement 346-907.{{photo1}} ]] | |||
=SEM Supra 1= | |||
The SEM Supra 1 is a scanning electron microscope (SEM). It produces enlarged images of a variety of specimens, achieving magnifications of over 500.000x providing ultra high resolution imaging. This important and widely used analytical tool provides exceptional resolution and depth of field, and minimal specimen preparation is required. | |||
This SEM is equipped two secondary electron (SE) detectors: An SE2 detector located on one side inside the chamber and an Inlens detector located inside the column. The SEM also has a backscatter electron detector: A BSD detector | |||
The SEM is a VP (variable pressure) instrument - Indicating that it is capable of operating at variable pressure. By increasing the pressure in the chamber and using a dedicated VPSE (Variable Pressure Secondary Electron) detector it is possible to image isolating samples. The higher density of gas molecules will eliminate the charges at the cost of slightly reduced resolution. Also, the SE2 and InLens detectors will no longer work. | |||
The SEM is the training for fabrication SEM at DTU Nanolab. It means that all new SEM users with no or little SEM experience must be trained on this tool and gain basic knowledge here before being qualified for training on other SEM's. | |||
The SEM Supra 1 was installed in the cleanroom in November 2010, but it has now been relocated in the basement outside the cleanroom, so that users can avoid to clean samples that have been outside the cleanroom before SEM inspection. | |||
The SEM | The Sputter Coater 03 is located in the same room as the SEM Supra 1 and can be used to cover non-conductive samples (for instance glass or polymer samples) with a thin gold layer before SEM inspection to avoid charging problems. | ||
Only users with samples that are somehow related to the work taking place in building 346 and 347 (the characterization part of DTU Nanolab). Other users will have to use the SEMs in building 314 (the characterization part of DTU Nanolab). | |||
'''The user manual, control instruction, the user APV and contact information can be found in LabManager:''' | '''The user manual, control instruction, the user APV and contact information can be found in LabManager:''' | ||
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach= | [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=275 SEM Supra 1 info page in LabManager], | ||
| Line 26: | Line 33: | ||
*[[Specific Process Knowledge/Characterization/SEM: Scanning Electron Microscopy|SEM comparison page]] | *[[Specific Process Knowledge/Characterization/SEM: Scanning Electron Microscopy|SEM comparison page]] | ||
==Equipment performance | ==Equipment performance== | ||
{| border="2" cellspacing="0" cellpadding="2" | {| border="2" cellspacing="0" cellpadding="2" | ||
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment | !colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment | ||
|style="background:WhiteSmoke; color:black"|<b>SEM | |style="background:WhiteSmoke; color:black"|<b>SEM Supra 1 (Supra 40VP SEM)</b> | ||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan=" | !style="background:silver; color:black" align="center" valign="center" rowspan="1"|Purpose | ||
|style="background:LightGrey; color:black"|Imaging and measurement of | |style="background:LightGrey; color:black"|Imaging and measurement of | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | * Conducting samples | ||
* Semi-conducting samples | |||
* Thin (~ 5 µm <) layers of non-conducting materials such as polymers | |||
* Thick polymers, glass or quartz samples | |||
* | |||
|- | |- | ||
!style="background:silver; color:black;" align="center" width="60"|Location | !style="background:silver; color:black;" align="center" width="60"|Location | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Basement of building 346 | ||
|- | |- | ||
!style="background:silver; color:black;" align="center" width="60"|Performance | !style="background:silver; color:black;" align="center" width="60"|Performance | ||
|style="background:LightGrey; color:black"|Resolution | |style="background:LightGrey; color:black"|Resolution | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *1-2 nm (limited by vibrations) | ||
The resolution is strongly dependent on the type of sample and the skills of the operator. | The resolution is strongly dependent on the type of sample and the skills of the operator. | ||
|- | |- | ||
| Line 60: | Line 65: | ||
*Secondary electron (Se2) | *Secondary electron (Se2) | ||
*Inlens secondary electron (Inlens) | *Inlens secondary electron (Inlens) | ||
*Backscatter electron ( | *4 Quadrant Backscatter electron (QBSD) | ||
*Variable pressure secondary electron (VPSE) | |||
|- | |- | ||
|style="background:LightGrey; color:black"|Stage | |style="background:LightGrey; color:black"|Stage | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*X, Y: | *X, Y: 130 × 130 mm | ||
*T: | *T: -4 to 70<sup>o</sup> | ||
*R: 360<sup>o</sup> | *R: 360<sup>o</sup> | ||
*Z: | *Z: 50 mm | ||
|- | |- | ||
|style="background:LightGrey; color:black"|Electron source | |style="background:LightGrey; color:black"|Electron source | ||
| Line 75: | Line 81: | ||
|style="background:LightGrey; color:black"|Operating pressures | |style="background:LightGrey; color:black"|Operating pressures | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Fixed at High vacuum (2 × 10<sup>- | *Fixed at High vacuum (2 × 10<sup>-4</sup>mbar - 10<sup>-6</sup>mbar) | ||
*Variable at Low vacuum (0.1 mbar - 2 mbar) | |||
|- | |- | ||
|style="background:LightGrey; color:black"|Options | |style="background:LightGrey; color:black"|Options | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *All software options available | ||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates | !style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates | ||
|style="background:LightGrey; color:black"|Batch size | |style="background:LightGrey; color:black"|Batch size | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *Up to 6" wafer with full view | ||
|- | |- | ||
| style="background:LightGrey; color:black"|Allowed materials | | style="background:LightGrey; color:black"|Allowed materials | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Any standard cleanroom | *Any standard cleanroom material and samples from the Laser Micromachining tool and the Polymer Injection Molding tool | ||
|- | |- | ||
|} | |||
===Quality control of length measurement === | |||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality Control (QC) for SEM Supra 1''' | |||
|- | |||
| | |||
*[http://labmanager.dtu.dk/d4Show.php?id=2493&mach=275 QC procedure for SEM Supra 1]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=275 Newest QC data for SEM Supra 1]<br> | |||
'''QC limits:''' | |||
{| {{table}} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px" | |||
! Detector | |||
! Settings | |||
! Magnification | |||
! Measured dimensions | |||
! Calibration limit | |||
! Action limit | |||
|- | |||
|SE2 | |||
| EHT 10 kV, WD 10 mm | |||
| 2.500 k | |||
| 70x70 μm | |||
| ± 2 % | |||
| ± 3 % | |||
|- | |||
|SE2 | |||
| EHT 10 kV, WD 10 mm | |||
| 17.000 k | |||
| 10x10 μm | |||
| ± 2 % | |||
| ± 3 % | |||
|- | |||
|SE2 | |||
| EHT 5 kV, WD 5 mm | |||
| 17.000 k | |||
| 10x10 μm | |||
| ± 2 % | |||
| ± 3 % | |||
|- | |||
| VPSE | |||
| EHT 10 kV, WD 10 mm, 17 Pa | |||
| 17.000 k | |||
| 10x10 μm | |||
| ± 2 % | |||
| ± 3 % | |||
|- | |||
| InLens | |||
| EHT 5 kV, WD 5 mm | |||
| 200.000 k | |||
| 1x1 μm | |||
| ± 2 % | |||
| ± 3 % | |||
|- | |||
| InLens | |||
| EHT 10 kV, WD 3 mm | |||
| 1.000.000 k | |||
| (imaging only) | |||
| NA | |||
| NA | |||
|- | |||
|} | |||
|- | |||
|} | |||
|} | |} | ||
Latest revision as of 15:54, 4 August 2025
Feedback to this page: click here
This page is written by DTU Nanolab internal

SEM Supra 1
The SEM Supra 1 is a scanning electron microscope (SEM). It produces enlarged images of a variety of specimens, achieving magnifications of over 500.000x providing ultra high resolution imaging. This important and widely used analytical tool provides exceptional resolution and depth of field, and minimal specimen preparation is required.
This SEM is equipped two secondary electron (SE) detectors: An SE2 detector located on one side inside the chamber and an Inlens detector located inside the column. The SEM also has a backscatter electron detector: A BSD detector
The SEM is a VP (variable pressure) instrument - Indicating that it is capable of operating at variable pressure. By increasing the pressure in the chamber and using a dedicated VPSE (Variable Pressure Secondary Electron) detector it is possible to image isolating samples. The higher density of gas molecules will eliminate the charges at the cost of slightly reduced resolution. Also, the SE2 and InLens detectors will no longer work.
The SEM is the training for fabrication SEM at DTU Nanolab. It means that all new SEM users with no or little SEM experience must be trained on this tool and gain basic knowledge here before being qualified for training on other SEM's.
The SEM Supra 1 was installed in the cleanroom in November 2010, but it has now been relocated in the basement outside the cleanroom, so that users can avoid to clean samples that have been outside the cleanroom before SEM inspection.
The Sputter Coater 03 is located in the same room as the SEM Supra 1 and can be used to cover non-conductive samples (for instance glass or polymer samples) with a thin gold layer before SEM inspection to avoid charging problems.
Only users with samples that are somehow related to the work taking place in building 346 and 347 (the characterization part of DTU Nanolab). Other users will have to use the SEMs in building 314 (the characterization part of DTU Nanolab).
The user manual, control instruction, the user APV and contact information can be found in LabManager:
SEM Supra 1 info page in LabManager,
Performance information
Equipment performance
| Equipment | SEM Supra 1 (Supra 40VP SEM) | |
|---|---|---|
| Purpose | Imaging and measurement of |
|
| Location |
| |
| Performance | Resolution |
The resolution is strongly dependent on the type of sample and the skills of the operator. |
| Instrument specifics | Detectors |
|
| Stage |
| |
| Electron source |
| |
| Operating pressures |
| |
| Options |
| |
| Substrates | Batch size |
|
| Allowed materials |
| |
Quality control of length measurement
| Quality Control (QC) for SEM Supra 1 | |||||||||||||||||||||||||||||||||||||||||||
|
QC limits:
|