Specific Process Knowledge/Etch/Wet Silicon Nitride Etch: Difference between revisions
No edit summary |
Only spelling |
||
| (27 intermediate revisions by 6 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Silicon_Nitride_Etch click here]''' | |||
''' | '''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.''' | ||
'''All links to Kemibrug (SDS) and Labmanager Including APV requires login.''' | |||
[[ | |||
'''All measurements on this page has been made by Nanolab staff.''' | |||
[[index.php?title=Category:Equipment|Etch Wet silicon nitride]] | |||
[[index.php?title=Category:Etch (Wet) bath|Silicon Nitride]] | |||
[[Image:Nitrideetch.JPG|300x300px|thumb|The 'Nitride etch' bath is placed inside 'Wet bench 02: Nitride ethc' in Cleanroom D-3]] | |||
Wet Etching of silicon nitride - stoichiometric and Si-rich - is done in a dedicated wetbench with an integrated quartz tank. The quartz tank can take up to 25 6" wafers in dedicated carriers. The 'Wetbench 02: Nitride etch' is placed in cleanroom D-3. The process is mainly used to strip silicon nitride (maskless), but can also be used for masked etching of silicon nitride using some kind of silicon oxide as etch mask. However, the wet silicon nitride etch is isotropic - meaning that the under-etching (etch-bias) at least amounts to the thickness of the silicon nitride layer. | |||
The etch solution is initially 85 wt% H<sub>3</sub>PO<sub>4</sub> which is heated up to the boiling temperature - approx. 160°C. | |||
'''NB: Great care has to be taken in this process due to risk of bumping. Therefore it is essential, that you stir thoroughly during heat up, before you start heating, at 50°C, 80°C and finally at 100°C''' | |||
'''The user | '''The user manual, user APV and contact information can be found in LabManager:''' | ||
<!-- remember to remove the type of documents that are not present --> | <!-- remember to remove the type of documents that are not present --> | ||
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=377 Nitride etch info page in LabManager], | |||
[ | |||
<br clear="all" /> | <br clear="all" /> | ||
== | ==Wet Silicon Nitride Etch== | ||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | ||
| Line 31: | Line 38: | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
! | ! | ||
! Nitride Etch @ 160<sup>o</sup>C | |||
! Nitride Etch @ 160 <sup>o</sup>C | |||
|- | |- | ||
| Line 38: | Line 44: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Generel description | !Generel description | ||
|Etch/strip of silicon nitride | |Etch/strip of silicon nitride | ||
|- | |- | ||
| Line 44: | Line 49: | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Link to safety APV and | !Link to safety APV and SDS | ||
|[http://labmanager.danchip.dtu.dk/d4Show.php?id=1892&mach=130 see APV here] | |[http://labmanager.danchip.dtu.dk/d4Show.php?id=1892&mach=130 see APV here] | ||
[ | [https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESk1OTEZKTVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K see SDS here (requires login)] | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Chemical solution | !Chemical solution | ||
|H<sub>3</sub>PO<sub>4</sub> (85 wt%) | |H<sub>3</sub>PO<sub>4</sub> (85 wt%) | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Process temperature | !Process temperature | ||
|160 <sup>o</sup>C | |160 <sup>o</sup>C | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
|'''Possible masking materials''' | |'''Possible masking materials''' | ||
| | | | ||
*Thermal oxide (converted si-rich surface) | *Thermal oxide (converted si-rich surface) | ||
| Line 73: | Line 70: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Etch rate | !Etch rate | ||
| | | | ||
*~26 Å/min (Si-rich Si<sub>3</sub>N<sub>4</sub>) | *~26 Å/min (Si-rich Si<sub>3</sub>N<sub>4</sub>) | ||
| Line 83: | Line 75: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Selectivity R<sub>Si<sub>3</sub>N<sub>4</sub></sub> / R<sub>SiO<sub>2</sub></sub> | !Selectivity R<sub>Si<sub>3</sub>N<sub>4</sub></sub> / R<sub>SiO<sub>2</sub></sub> | ||
|The selectivity (sirich nitride:oxide) is higher at 160 <sup>o</sup>C than at 180 <sup>o</sup>C | |The selectivity (sirich nitride:oxide) is higher at 160 <sup>o</sup>C than at 180 <sup>o</sup>C | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Batch size | !Batch size | ||
| | | | ||
1-25 wafer at a time | 1-25 wafer at a time | ||
| Line 95: | Line 84: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Size of substrate | !Size of substrate | ||
| | | | ||
2-6" wafers | 2-6" wafers | ||
| Line 102: | Line 89: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Allowed materials | !Allowed materials | ||
| | | | ||
*Silicon | *Silicon | ||
Latest revision as of 09:14, 31 July 2025
Feedback to this page: click here
Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.
All links to Kemibrug (SDS) and Labmanager Including APV requires login.
All measurements on this page has been made by Nanolab staff.
Etch Wet silicon nitride Silicon Nitride
Wet Etching of silicon nitride - stoichiometric and Si-rich - is done in a dedicated wetbench with an integrated quartz tank. The quartz tank can take up to 25 6" wafers in dedicated carriers. The 'Wetbench 02: Nitride etch' is placed in cleanroom D-3. The process is mainly used to strip silicon nitride (maskless), but can also be used for masked etching of silicon nitride using some kind of silicon oxide as etch mask. However, the wet silicon nitride etch is isotropic - meaning that the under-etching (etch-bias) at least amounts to the thickness of the silicon nitride layer.
The etch solution is initially 85 wt% H3PO4 which is heated up to the boiling temperature - approx. 160°C.
NB: Great care has to be taken in this process due to risk of bumping. Therefore it is essential, that you stir thoroughly during heat up, before you start heating, at 50°C, 80°C and finally at 100°C
The user manual, user APV and contact information can be found in LabManager:
Nitride etch info page in LabManager,
Wet Silicon Nitride Etch
| Nitride Etch @ 160oC | |
|---|---|
| Generel description | Etch/strip of silicon nitride |
| Link to safety APV and SDS | see APV here |
| Chemical solution | H3PO4 (85 wt%) |
| Process temperature | 160 oC |
| Possible masking materials |
|
| Etch rate |
|
| Selectivity RSi3N4 / RSiO2 | The selectivity (sirich nitride:oxide) is higher at 160 oC than at 180 oC |
| Batch size |
1-25 wafer at a time |
| Size of substrate |
2-6" wafers |
| Allowed materials |
|