=Niobium Titanium (NbTi)= | |||
Niobium–titanium (Nb‑Ti) is a ductile, readily machinable alloy that merges niobium’s superconductivity with titanium’s strength, yielding a rigid, corrosion‑resistant material valued in cryogenic and high‑field environments. | Niobium–titanium (Nb‑Ti) is a ductile, readily machinable alloy that merges niobium’s superconductivity with titanium’s strength, yielding a rigid, corrosion‑resistant material valued in cryogenic and high‑field environments. | ||
| Line 11: | Line 18: | ||
Users can deposit NbTi in either the Sputter-System (Lesker) or the Sputter-System Metal-Nitride(PC3) (Preferable option) | Users can deposit NbTi in either the Sputter-System (Lesker) or the Sputter-System Metal-Nitride(PC3) (Preferable option) | ||
* [[Specific Process Knowledge/Thin film deposition/Deposition of NbTi/Deposition of NbTi in Sputter-System Metal-Nitride PC3 | * [[Specific Process Knowledge/Thin film deposition/Deposition of NbTi/Deposition of NbTi in Sputter-System Metal-Nitride PC3|Deposition of NbTi in Sputter-System Metal-Nitride(PC3)]] | ||
==Comparison of sputter systems for alloy deposition== | ==Comparison of sputter systems for alloy deposition== | ||
| Line 39: | Line 46: | ||
!Stoichiometry | !Stoichiometry | ||
| | | | ||
*NbTi (Sputter-System Metal-Nitride(PC3)) | *NbTi (Sputter-System Metal-Nitride(PC3)) NbTi 67/33 At.% (4" target) | ||
| | | | ||
*Unknown | *Unknown | ||
| Line 63: | Line 69: | ||
*Up to 600 °C | *Up to 600 °C | ||
| | | | ||
*Up to 400 °C | *Up to 400 °C (Room temperature from 2021) | ||
|- | |- | ||
Latest revision as of 17:32, 30 July 2025
Feedback to this page: click here
Unless otherwise stated, this page is written by DTU Nanolab internal
Niobium Titanium (NbTi)
Niobium–titanium (Nb‑Ti) is a ductile, readily machinable alloy that merges niobium’s superconductivity with titanium’s strength, yielding a rigid, corrosion‑resistant material valued in cryogenic and high‑field environments. Thin films are produced chiefly by magnetron sputtering, where the Nb/Ti ratio and post‑anneal determine phase purity, resistivity, and the superconducting critical temperature (≈ 9.2 K for near‑eutectic compositions). In microelectronics, Nb‑Ti can act as a robust diffusion barrier, gate or contact metal, and mechanically compliant liner. Yet, its signature role is as a superconductor: kilometer-length multifilament Nb-Ti wires carry mega-ampere currents in MRI scanners, particle-accelerator magnets, and experimental fusion coils under magnetic fields approaching 10 T. Ultrathin Nb‑Ti nanowires serve in superconducting nanowire single‑photon detectors, kinetic‑inductance detectors, and low‑loss microwave resonators, while Nb‑Ti/Al bilayers enable Josephson junctions and rapid single‑flux‑quantum circuits. The alloy’s radiation tolerance, thermal stability, and moderate atomic number support cryogenic beam‑line components and X‑ray filters, and its biocompatibility and wear resistance extend its usefulness to medical implants and protective MEMS coatings, underscoring Nb‑Ti’s versatility wherever robust, easily processed superconducting or barrier films are required.
Sputter deposition of Niobium Nitride
Users can deposit NbTi in either the Sputter-System (Lesker) or the Sputter-System Metal-Nitride(PC3) (Preferable option)
Comparison of sputter systems for alloy deposition
| Sputter-System Metal-Nitride(PC3) | Lesker sputter system | |
|---|---|---|
| Generel description |
|
|
| Stoichiometry |
|
|
| Film thickness |
|
|
| Process temperature |
|
|
| Step coverage |
|
|
| Film quality |
|
|
| Batch size |
|
|
| Allowed materials |
|
|