Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of ITO: Difference between revisions

From LabAdviser
Reet (talk | contribs)
Eves (talk | contribs)
No edit summary
 
(11 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_ITO click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_ITO click here]'''


''All contents by DTU Nanolab staff.''
=Indium tin oxide (ITO)=
Indium tin oxide (ITO) is the canonical degenerate n‑type transparent conducting oxide, combining high visible transmittance with low sheet resistance and a mature, scalable manufacturing base.
It is deposited industrially by magnetron sputtering for uniform, low-resistivity films. ITO is the workhorse transparent electrode for displays and touch panels, OLED/LED emitters, and a wide range of photovoltaic technologies; oxygen stoichiometry is tuned to balance conductivity and transparency.
In photonics, heavily doped ITO exhibits an epsilon-near-zero response in the near-infrared (around the 1.55 µm telecom band), enabling compact electro-optic modulators, plasmonic waveguides, and absorbers, as well as strong nonlinear/ultrafast effects.
ITO can also become superconducting at cryogenic temperatures when strongly reduced or ion-intercalated, with reported critical temperatures ranging from sub-kelvin to a few kelvin, depending on the carrier density and processing.
Beyond semiconductors and optics, ITO supports transparent heaters, low-emissivity and EMI-shielding window coatings, and ENZ-enabled NIR photodetectors. When even lower resistance is required, it is often paired with ultrathin metals in hybrid stacks, while retaining high transparency.


==Deposition of ITO==
==Deposition of ITO==
ITO (indium tin oxide) can be deposited by sputtering here at Nanolab. An ITO target is used and it may be sputtered either non-reactively in Ar or reactively in a mixture of Ar and O<sub>2</sub>.
ITO (indium tin oxide) can be deposited by sputtering here at DTU Nanolab. An ITO target is used and it may be sputtered either non-reactively in Ar or reactively in a mixture of Ar and O<sub>2</sub>.


*[[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|Deposition conditions and a few results]] for ITO deposited for the acceptance test of the Sputter-System Metal-Oxide(PC1)
We have acquired a lot of knowledge about ITO deposition in our Cluster Lesker system, and results are summarized on a page here:
 
*[[Specific_Process_Knowledge/Thin_film_deposition/Deposition of ITO/Sputtering of ITO in Sputter-System Metal-Oxide (PC1)|Sputtering of ITO in Sputter-System Metal-Oxide (PC1)]].


==Comparison of the methods for deposition of ITO==
==Comparison of the methods for deposition of ITO==
Line 24: Line 36:
*RF sputtering of an ITO target - reactive sputtering possible
*RF sputtering of an ITO target - reactive sputtering possible
|
|
*RF sputtering of an ITO target - reactive sputtering possible
*RF sputtering of an ITO target - reactive sputtering possible (not recommended due to arching)
*Pulsed DC sputtering of an ITO target - reactive sputtering possible
*Pulsed DC sputtering of an ITO target - reactive sputtering possible
*Reactive HIPIMS (high-power impulse magnetron sputtering) of an ITO target
|-
|-


Line 35: Line 46:
*Not known
*Not known
|
|
*In:Sn:O ~ 39:3:58 in the [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Process information|acceptance test]]. Can be tuned by altering deposition conditions.
*In:Sn:O ~ 39:3:58. Can be tuned by altering [[Specific_Process_Knowledge/Thin_film_deposition/Deposition of ITO/Sputtering of ITO in Sputter-System Metal-Oxide (PC1)#Stoichiometry|deposition conditions]].
|-
|-


Line 53: Line 64:
* 0.5-2 nm/min
* 0.5-2 nm/min
|
|
* at least up to ~ 12 nm/min ([[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|see conditions]])
* at least up to ~ 10 nm/min ([[Specific_Process_Knowledge/Thin_film_deposition/Deposition of ITO/Sputtering of ITO in Sputter-System Metal-Oxide (PC1)#Deposition_rate|see conditions]])
|-
|-


Line 68: Line 79:
!Process Temperature
!Process Temperature
|
|
* Up to 400 °C
* Up to 400 °C (tool limit)
|
|
* Up to 600 °C
* Up to 600 °C (tool limit)
|-
|-



Latest revision as of 16:37, 28 July 2025

Feedback to this page: click here

All contents by DTU Nanolab staff.


Indium tin oxide (ITO)

Indium tin oxide (ITO) is the canonical degenerate n‑type transparent conducting oxide, combining high visible transmittance with low sheet resistance and a mature, scalable manufacturing base. It is deposited industrially by magnetron sputtering for uniform, low-resistivity films. ITO is the workhorse transparent electrode for displays and touch panels, OLED/LED emitters, and a wide range of photovoltaic technologies; oxygen stoichiometry is tuned to balance conductivity and transparency. In photonics, heavily doped ITO exhibits an epsilon-near-zero response in the near-infrared (around the 1.55 µm telecom band), enabling compact electro-optic modulators, plasmonic waveguides, and absorbers, as well as strong nonlinear/ultrafast effects. ITO can also become superconducting at cryogenic temperatures when strongly reduced or ion-intercalated, with reported critical temperatures ranging from sub-kelvin to a few kelvin, depending on the carrier density and processing. Beyond semiconductors and optics, ITO supports transparent heaters, low-emissivity and EMI-shielding window coatings, and ENZ-enabled NIR photodetectors. When even lower resistance is required, it is often paired with ultrathin metals in hybrid stacks, while retaining high transparency.

Deposition of ITO

ITO (indium tin oxide) can be deposited by sputtering here at DTU Nanolab. An ITO target is used and it may be sputtered either non-reactively in Ar or reactively in a mixture of Ar and O2.

We have acquired a lot of knowledge about ITO deposition in our Cluster Lesker system, and results are summarized on a page here:

Comparison of the methods for deposition of ITO

Sputter-System(Lesker) Sputter-System Metal-Oxide(PC1)
Generel description
  • RF sputtering of an ITO target - reactive sputtering possible
  • RF sputtering of an ITO target - reactive sputtering possible (not recommended due to arching)
  • Pulsed DC sputtering of an ITO target - reactive sputtering possible
Stoichiometry
  • Not known
Film Thickness
  • few nm - ~ 200 nm
  • few nm - ~ 1 μm
Deposition rate
  • 0.5-2 nm/min
Step coverage
  • unknown
  • unknown
Process Temperature
  • Up to 400 °C (tool limit)
  • Up to 600 °C (tool limit)
Substrate size
  • chips
  • 1x 100 mm wafer
  • 1x 150 mm wafer
  • chips
  • 10x 100 mm wafer
  • 10x 150 mm wafer
Allowed materials
  • almost any