====Etch rate & uniformity====
====Etch rate & uniformity====


'''Recipe: ''Slowetch 2'''''


'''SRN (LPCVD) etch uniformity on 6″ wafer with ''Slowetch 2'' recipe'''
'''SRN (LPCVD) etch uniformity on 6″ wafer'''
[[File:slowetch2_100% loadSRN.png|400px|left|thumb|Process: No mask, 100 % load, etching was done after 10 mins chamber clean + 5 mins TDESC clean (for all wafers)]]
[[File:slowetch2_100% loadSRN.png|400px|left|thumb|Process: No mask, 100 % load, etching was done after 10 mins chamber clean + 5 mins TDESC clean (for all wafers)]]
[[File:slowetch2_100% loadSRN_etchrate.png|400px|left|thumb|Note: etch rate for SRN with Slowetch 2. The 4 wafers were processed on 4 different days,  the variation suggests process instability or chamber memory effects influencing etch behavior across runs.]]
[[File:slowetch2_100% loadSRN_etchrate.png|400px|left|thumb|Note: etch rate for SRN with Slowetch 2. The 4 wafers were processed on 4 different days,  the variation suggests process instability or chamber memory effects influencing etch behavior across runs.]]
Line 82: Line 83:


<br clear="all" />
<br clear="all" />
'''SRN (LPCVD) etch uniformity on 6″ wafer with ''Slowetch'' recipe'''
 
'''Recipe: ''Slowetch'''''
 
'''SRN (LPCVD) etch uniformity on 6″ wafer '''


[[File:SRN_slowetch_data_100%load.png|400px|left|thumb|Process: No mask, 100 % load, etching was done after 10 mins chamber clean + 5 mins TDESC clean (for all wafers)<br/>
[[File:SRN_slowetch_data_100%load.png|400px|left|thumb|Process: No mask, 100 % load, etching was done after 10 mins chamber clean + 5 mins TDESC clean (for all wafers)<br/>
Line 88: Line 92:




<br clear="all" />


 
'''With DUV mask on ~300 nm SRN layer'''
[[File:SRN_slowetch_profilealong center.png|800px|left|thumb|Process: ''Slowetch recipe for 10 mins'', DUV mask (with Barc) ~750 nm, etching was done after 10 mins chamber clean + 5 mins TDESC clean (for all wafers)<br/>
Note: The SEM images illustrate the etched SRN profiles across the wafer, progressing from one edge (left) through the center chip (middle) to the opposite edge (right), the etch rate is ~28 nm/min.]]