Jump to content

Specific Process Knowledge/Etch/KOH Etch/ProcessInfo: Difference between revisions

Kabi (talk | contribs)
Mbec (talk | contribs)
 
(13 intermediate revisions by one other user not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/KOH_Etch/ProcessInfo click here]'''
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/KOH_Etch/ProcessInfo click here]'''
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''
'''All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.'''


==QC==
==QC==
===Quality Control (QC) for the KOH Si etching baths.===
===Quality Control (QC) for the KOH Si etching baths.===
''All links in the table below reguire login to labmanager**
'''All links in the table below reguire login to labmanager'''
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Control (QC) for Si Etch 01, and Si Etch 02'''
|bgcolor="#98FB98" |'''Quality Control (QC) for Si Etch 01, and Si Etch 02'''
Line 11: Line 16:
*[http://labmanager.dtu.dk/d4Show.php?id=5476&mach=407 The QC procedure for Si Etch: 03]<br>
*[http://labmanager.dtu.dk/d4Show.php?id=5476&mach=407 The QC procedure for Si Etch: 03]<br>
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:200px"
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:200px"


Line 25: Line 30:
|Time
|Time
|90 min
|90 min
|-
|Elevator
|On
|-
|-
|Substrate
|Substrate
Line 77: Line 79:


<math>X=\frac{(Y\cdot 1000g)}{(1.509g/ml\cdot(0.5-Y))}</math>
<math>X=\frac{(Y\cdot 1000g)}{(1.509g/ml\cdot(0.5-Y))}</math>




Line 96: Line 99:
Due to the almost inert (111)-planes it is possible by KOH etching to realize high aspect ratio structures in sigle crytalline silicon using the (111)-planes as sidewalls. In Si(100) these sidewalls are inclined - 54.7<sup>o</sup> with respect to the (100) surface - whereas in Si(110) the sidewalls are vertical (see figures below).
Due to the almost inert (111)-planes it is possible by KOH etching to realize high aspect ratio structures in sigle crytalline silicon using the (111)-planes as sidewalls. In Si(100) these sidewalls are inclined - 54.7<sup>o</sup> with respect to the (100) surface - whereas in Si(110) the sidewalls are vertical (see figures below).


<gallery caption="Anisotropic wet silicon etch: dependency on crystal orientation" widths="380px" heights="150px" perrow="2">  
<gallery caption="Anisotropic wet silicon etch: dependency on crystal orientation" widths="760px" heights="150px" perrow="1">  
Image:KOH_Anisotropy.jpg|Etched profile when etching Si(100).
 
Image:KOH_Anisotropy(110).jpg|Etched profile when etching Si(110).
Image:KOH-etch.JPG|Etched profile when etching Si(100) and when etching Si(110) respectively
 
<!-- Image:KOH_Anisotropy.jpg|Etched profile when etching Si(100).-->
<!-- Image:KOH_Anisotropy(110).jpg|Etched profile when etching Si(110).-->
</gallery>
</gallery>


<br clear="all"/>
<br clear="all"/>
For Si(100), the relation between the width of the bottom of the etched groove (W<sub>b</sub>) and the width of the opening (W<sub>o</sub>) at the wafer surface in a groove etched to the depth l is given by:
For Si(100), the relation between the width of the bottom of the etched groove (W<sub>b</sub>) and the width of the opening (W<sub>o</sub>) at the wafer surface in a groove etched to the depth d is given by:
 


<math>W_b = W_o - 2d cot(54.7^o) = W_o - \sqrt{2} d</math>


<math>W_b = W_o - 2lcot(54.7^o) = W_o - \sqrt{2} l</math>




Line 112: Line 119:
===Definition of <110> alignment structures===
===Definition of <110> alignment structures===


The etch rate dependence on the crystallographic planes can be used to determine the <110> crystal directions with high precision (better than +/- 0.05 <sup>o</sup>). A fast method for doing this, using the symmetric under-cutting behavior around but not at the <110>-directions, was described by https://iopscience.iop.org/article/10.1088/0960-1317/6/2/011/meta. [[https://iopscience.iop.org/article/10.1088/0960-1317/6/2/011/meta|Mattias Vangbo and Ylva Bäcklund 1996 J. Micromech. Microeng. '''6''', 279-284]]  High-precision control of the <110>-direction during alignment can be necessary in order to control the dimensions of KOH-etched structures (e.g. precise control of V-groove dimensions).  
The etch rate dependence on the crystallographic planes can be used to determine the <110> crystal directions with high precision (better than +/- 0.05 <sup>o</sup>). A fast method for doing this, using the symmetric under-cutting behavior around but not at the <110>-directions, was described by [https://iopscience.iop.org/article/10.1088/0960-1317/6/2/011/meta Mattias Vangbo and Ylva Bäcklund 1996 J. Micromech. Microeng. '''6''', 279-284]. High-precision control of the <110>-direction during alignment can be necessary in order to control the dimensions of KOH-etched structures (e.g. precise control of V-groove dimensions).  
 


<br clear="all" />
<br clear="all" />


===Etch rates: Empirical formula (Seidl et al)===
<!-- ===Etch rates: Empirical formula (Seidl et al)===


The following empirical formula can be used for concentrations in the range of 10-60 wt%:
The following empirical formula can be used for concentrations in the range of 10-60 wt%:
Line 125: Line 131:
where k<sub>0</sub> = 2480 µm/hr (mol/l)<sup>-4.25</sup>, E<sub>a</sub> = 0.595 eV for Si(100)
where k<sub>0</sub> = 2480 µm/hr (mol/l)<sup>-4.25</sup>, E<sub>a</sub> = 0.595 eV for Si(100)


and  k<sub>0</sub> = 4500 µm/hr (mol/l)<sup>-4.25</sup>, E<sub>a</sub> = 0.60 eV for Si(110)
and  k<sub>0</sub> = 4500 µm/hr (mol/l)<sup>-4.25</sup>, E<sub>a</sub> = 0.60 eV for Si(110) -->