Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of TiW: Difference between revisions

Kn (talk | contribs)
No edit summary
Reet (talk | contribs)
 
(20 intermediate revisions by 5 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:pvd@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_TiW&action=edit click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_TiW click here]'''  


<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b></i>


Deposition of TiW alloy can take place in the Wordentec.
==Sputtering of TiW==


Deposition of TiW alloy was done in the past in the [[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]]. This tool is now decommissioned, and if necessary processes may be developed for depositing TiW in the Lesker sputter setups (contact responsible staff for this).


{| border="1" cellspacing="0" cellpadding="4"
*[[/Sputtering of TiW in Wordentec|Sputtering of TiW in Wordentec]]
!
*[[Specific Process Knowledge/Thin film deposition/Deposition of TiW/Sputtering of TiW in Wordentec/Grain size and uniformity of TiW layers|Results of a study on the grain size and uniformity of TiW sputtered in the Wordentec]]
! Sputter deposition (Wordentec)
|-
| Batch size
|
*24x2" wafers or
*6x4" wafers or
*6x6" wafers
|-
| Pre-clean
|RF Ar clean
|-
| Layer thickness
|.
|-
| Deposition rate
|Depending on process parameters, see [[/Sputtering of TiW in Wordentec|here.]]
|-
|}
 
 
'''Deposited rates'''
 
This is done by a sputtering process. Process parameters (argon pressure and effect) can be varied, the surface roughness and the deposition rate (see [[/Sputtering of TiW in Wordentec|here]]) and may change with these settings.
 
 
'''Deposited film characteristics'''
 
AFM pictures show how the surface roughness is dependent of the process parameters, this can be seen here.