Line 71: Line 71:


|
|
*Almost any that does not degas at your intended substrate temperature. See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet]
*Almost any that does not degas at your intended substrate temperature. See also the [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet]
|
|
* Almost any that do not degas.
* Almost any that do not degas. See also the [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=244 cross-contamination sheet]
|
|
*Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3]
*Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3]


|-
|-
Line 100: Line 100:
|-
|-
|
|
Nickel deposition is tested occasionally, around 1 time per year in each machine. You are welcome to contact staff to request an extra test of the material.


Nickel deposition is tested occasionally, around 1 time per year in each machine. Let us know if you notice any problems or would like an extra test of the material. LabManager links require login.
'''LabManager links to procedures and data''' (require login):


*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=429 QC procedure for the E-beam Evaporator (Temescal)]<br>
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=429 QC procedure for the E-beam Evaporator (Temescal)]<br>
Line 108: Line 109:
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=511 QC procedure for the E-beam Evaporator (10-pockets)]<br>
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=511 QC procedure for the E-beam Evaporator (10-pockets)]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=511 The newest QC data for the E-beam Evaporator (10-pockets)]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=511 The newest QC data for the E-beam Evaporator (10-pockets)]<br>


{| {{table}}
{| {{table}}
| align="left" |  
| align="left" valign="top"|
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:440px"
{| border="2" cellspacing="1" cellpadding="2" align="left" style="width:400px"
 
! QC Recipe:
! QC Recipe:
! Standard recipes/Ni  
! Standard recipes/Ni  
|-  
|-  
|Deposition rate
|Deposition rate
|10 Å/s
|2 Å/s
|-
|-
|Thickness
|Thickness
Line 124: Line 125:
|Pressure
|Pressure
|Below 1*10<sup>-6</sup> mbar
|Below 1*10<sup>-6</sup> mbar
|-
|}
|-
|-
|}
|}


{| {{table}}
{| {{table}}
| align="left" valign="top"|
| align="left" valign="top"|
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:440px"
{| border="2" cellspacing="1" cellpadding="2" align="left" style="width:400px"
!QC limits
!QC limits
!Both E-beam Evaporators
!Both E-beam Evaporators
Line 145: Line 149:
|-
|-
|}
|}
Thickness is measured in 5 points with a stylus profiler. <br>
 
Thickness is measured in 5 points with a stylus profiler (usually DektakXT). <br>
|}
|}

Latest revision as of 23:56, 7 July 2025

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here


Nickel deposition

Nickel can be deposited by e-beam evaporation or sputtering at DTU Nanolab. For electroplating you will have to contact other institutes at DTU, e.g., DTU Mechanical Engineering.

Some process information is available here for e-beam evaporated films:

In the chart below you can compare the different deposition equipment:

E-beam evaporation (E-beam evaporator (Temescal) and E-beam evaporator (10-pockets)) Sputter deposition (Lesker) Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3))
General description E-beam deposition of Nickel Sputter deposition of Nickel Sputter deposition of Nickel
Pre-clean Ar ion etch (only in E-beam evaporator Temescal) RF Ar clean
Layer thickness 10 Å to 1 µm * 10 Å to 500 nm ** 10 Å to 500 nm **
Deposition rate 1-10 Å/s Depends on process parameters, about 1 Å/s Depends on process parameters, at least ~ 4 Å/s, see conditions here
Batch size
  • Up to 4x6" wafers
  • Up to 3x8" wafers (ask for holder)
  • Many smaller pieces
  • Pieces or
  • 1x4" wafer or
  • 1x6" wafer
  • Up to 10x4" or 6" wafers
  • Many smaller pieces
Allowed materials
  • Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for PC1 and PC3
Comment
  • May use high-strength magnet for deposition.
  • May use high-strength magnet for deposition

* To deposit a cumulative thickness above 600 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine


** To deposit a cumulative thickness above 200 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine

Quality control of e-beam evaporated Ni films

Quality control (QC) for the E-beam Evaporator (Temescal) and the E-beam Evaporator (10-pockets)

Nickel deposition is tested occasionally, around 1 time per year in each machine. You are welcome to contact staff to request an extra test of the material.

LabManager links to procedures and data (require login):


QC Recipe: Standard recipes/Ni
Deposition rate 2 Å/s
Thickness 100 nm
Pressure Below 1*10-6 mbar


QC limits Both E-beam Evaporators
Deposition rate deviation ± 20 %
Measured average thickness ± 10 %
Thickness deviation across a 4" wafer ± 5 %

Thickness is measured in 5 points with a stylus profiler (usually DektakXT).