Specific Process Knowledge/Thin film deposition/Deposition of Palladium: Difference between revisions
Appearance
Took out Alcatel and replaced with Temescal |
|||
| (11 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto: | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Palladium&action=edit click here]''' | ||
<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b></i> | |||
===Palladium deposition=== | |||
Palladium can be deposited by e-beam evaporation or DC sputtering at DTU Nanolab. | |||
Palladium | ==Sputtering of Palladium== | ||
Palladium may be sputter deposited in the sputter-system (Lesker). See process results here: | |||
*[[/Pd sputtering in Sputter System (Lesker) |Pd sputtering in Sputter System (Lesker)]] | |||
==Equipment comparison== | |||
In the chart below you can compare the different deposition equipment: | |||
| Line 11: | Line 20: | ||
! | ! | ||
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|Temescal]]) | ! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|Temescal]] and [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]]) | ||
! | ! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System (Lesker)]]) | ||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]]) | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! General description | ! General description | ||
| E-beam deposition of Pd | | E-beam deposition of Pd | ||
| | | Sputter deposition of Pd | ||
| Sputter deposition of Pd | |||
|- | |- | ||
|-style="background:Lightgrey; color:black" | |-style="background:Lightgrey; color:black" | ||
! Pre-clean | ! Pre-clean | ||
|Ar ion source | |Ar ion source (only in E-beam Evaporator Temescal) | ||
|none | |||
|RF Ar clean | |RF Ar clean | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Layer thickness | ! Layer thickness | ||
|10 Å - | |10 Å - 600 nm* | ||
|10 Å | |10 Å - 600 nm* | ||
|Discuss with staff | |||
|- | |- | ||
|-style="background:Lightgrey; color:black" | |-style="background:Lightgrey; color:black" | ||
! Deposition rate | ! Deposition rate | ||
|0.5 Å/s to 10Å/s | |0.5 Å/s to 10Å/s | ||
| | |Up to 4.3 Å/s | ||
| Discuss with staff | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Batch size | ! Batch size | ||
| | | | ||
*Up to 4x6" wafers | *Up to 4x6" wafers | ||
*Up to 3x8" wafers | *Up to 3x8" wafers | ||
*smaller wafers and pieces | *smaller wafers and pieces | ||
| | | | ||
* | *1x4" wafer or | ||
* | *1x6" wafer or | ||
* | *several small samples | ||
| | |||
*Up to 10x4" or 6" wafers | |||
*Many smaller pieces | |||
|- | |- | ||
|-style="background:Lightgrey; color:black" | |-style="background:Lightgrey; color:black" | ||
!Allowed materials | !Allowed materials | ||
| | | | ||
* | *Almost any that does not degas | ||
*See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet] | *See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet] | ||
| | | | ||
* | *Almost any that does not degas. | ||
* | *See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=244 cross-contamination sheet] | ||
| Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3] | |||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Comment | ! Comment | ||
| | |||
| | | | ||
| | | | ||
| Line 70: | Line 81: | ||
|} | |} | ||
'''*''' ''If depositing more than 600 nm, please write to metal@ | '''*''' ''If depositing more than 600 nm, please write to metal@nanolab.dtu.dk well in advance to ensure that enough material is present.'' | ||
Latest revision as of 22:21, 7 July 2025
Feedback to this page: click here
Unless otherwise stated, this page is written by DTU Nanolab internal
Palladium deposition
Palladium can be deposited by e-beam evaporation or DC sputtering at DTU Nanolab.
Sputtering of Palladium
Palladium may be sputter deposited in the sputter-system (Lesker). See process results here:
Equipment comparison
In the chart below you can compare the different deposition equipment:
| E-beam evaporation (Temescal and E-beam evaporator (10-pockets)) | Sputter deposition (Sputter-System (Lesker)) | Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) | |
|---|---|---|---|
| General description | E-beam deposition of Pd | Sputter deposition of Pd | Sputter deposition of Pd |
| Pre-clean | Ar ion source (only in E-beam Evaporator Temescal) | none | RF Ar clean |
| Layer thickness | 10 Å - 600 nm* | 10 Å - 600 nm* | Discuss with staff |
| Deposition rate | 0.5 Å/s to 10Å/s | Up to 4.3 Å/s | Discuss with staff |
| Batch size |
|
|
|
| Allowed materials |
|
|
Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for PC1 and PC3 |
| Comment |
* If depositing more than 600 nm, please write to metal@nanolab.dtu.dk well in advance to ensure that enough material is present.