Jump to content

Specific Process Knowledge/Characterization/XRD: Difference between revisions

From LabAdviser
Khara (talk | contribs)
No edit summary
Reet (talk | contribs)
 
(40 intermediate revisions by 4 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Characterization/XRD click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Characterization/XRD click here]'''


=XRD at Nanolab=
<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b></i>
We have two X-ray diffraction setups in building 346:
 
*The [[/XRD_SmartLab|Rigaku SmartLab]] primarily for thin film analysis
 
*The [[/XRD_Powder|XRD Powder]] for phase analysis of powders
=XRD at DTU Nanolab=
We have three X-ray diffraction setups in building 346:
*The [[/XRD_SmartLab|XRD SmartLab]] primarily for thin film analysis inside the cleanroom.
*The [[/XRD SmartLab 9kW Rotating Anode|XRD SmartLab 9kW Rotating Anode]] multipurpose system outside the cleanroom.
*The [[/XRD_Powder|XRD Powder]] for phase analysis of powders outside the cleanroom.
 
==Experiments performed with XRD==
*[[/Process Info|List and description of possible XRD measurements with typical setup requirements]] Note mostly relevant for XRD Smartlab and XRD Rot Anode


==Data analysis==
==Data analysis==
For data analysis, we recommend using Rigaku SmartLab Studio for both thinfilms and basic powder analysis.
For data analysis, we recommend using Rigaku SmartLab Studio for both thinfilms and basic powder analysis.
If more advanced powder analysis is needed a remote desktop with a licens for the Malvern Panalytical software, HighScore is available.
If more advanced powder analysis is needed we provide access to a remote desktop with a licence for the excellent Malvern Panalytical software, HighScore.
 
*[[/software|Installing SmartLab Studio II]]
*[[/dataconversion|Converting data from XRD Powder to SmartLab Studio II]]
*[[/SLSII_analysis|Guide for using SmartLab Studio II for data analysis]]
*[[/HighScore_analysis|Guide for using HighScore Plus for advanced powder data analysis]]
*[[/XRD_Reference_Data|How to download reference spectra for individual crystal structures]] (for DTU users and others with access to the ICSD).


[[/software|Installing SmartLab Studio II]]
Apart from commercial software a wide range of free software is available online for data analysis. Please let us know if you find something you'd like to recommend!
[[SLSII_analysis|Guide for using SmartLab Studio II for data analysis]]


==Comparison of the XRDs at Nanolab==
==Comparison of the XRDs at Nanolab==
Line 19: Line 31:
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
|style="background:WhiteSmoke; color:black"|<b>XRD SmartLab</b>
|style="background:WhiteSmoke; color:black"|<b>XRD SmartLab</b>
|style="background:WhiteSmoke; color:black"|<b>XRD RotAnode</b>
|style="background:WhiteSmoke; color:black"|<b>XRD Powder</b>
|style="background:WhiteSmoke; color:black"|<b>XRD Powder</b>
|-
|-
!style="background:silver; color:black;" align="center" width="60"|Purpose  
!style="background:silver; color:black;" align="center" width="60"|Purpose  
|style="background:LightGrey; color:black"| Crystal structure analysis and thin film thickness measurement
|style="background:LightGrey; color:black"| Crystal structure analysis  
 
and thin film thickness measurement
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Phase ID
*Phase ID
Line 29: Line 44:
*Quality and degree of orientation
*Quality and degree of orientation
*3D orientation
*3D orientation
*Latice strain
*Lattice strain
*Composition
*Twist
*3D lattice constant
*Thickness
*Roughness
*Density
|style="background:WhiteSmoke; color:black"|
*Phase ID
*Crystal Size
*Crystallinity
*Quality and degree of orientation
*3D orientation
*Lattice strain
*Composition
*Composition
*Twist
*Twist
Line 46: Line 74:
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
3 kW
3 kW
|style="background:WhiteSmoke; color:black"|
9 kW
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
600 W
600 W
Line 51: Line 81:
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
Rated tube voltage
Rated tube voltage
|style="background:WhiteSmoke; color:black"|
20 to 45 kV
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
20 to 45 kV
20 to 45 kV
Line 60: Line 92:
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
2 to 60 mA
2 to 60 mA
|style="background:WhiteSmoke; color:black"|
2 to 200 mA
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
15 mA
15 mA
Line 67: Line 101:
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
Sealed tube
Sealed tube
|style="background:WhiteSmoke; color:black"|
Rotating Anode
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
Sealed tube
Sealed tube
Line 72: Line 108:
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
Target
Target
|style="background:WhiteSmoke; color:black"|
Cu
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
Cu
Cu
Line 81: Line 119:
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
0.4 mm x 8 mm (Line/Point)
0.4 mm x 8 mm (Line/Point)
|style="background:WhiteSmoke; color:black"|
0.1-0.5 mm x 8 mm (Line/Point)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
0.4 mm x 12 mm (Line)
0.4 mm x 12 mm (Line)
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="5"|Goniometer
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Goniometer
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
Scanning mode
Scanning mode
|style="background:WhiteSmoke; color:black"|
incident / receiver coupled or independent
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
incident / receiver coupled or independent
incident / receiver coupled or independent
Line 94: Line 136:
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
Goniomenter radius
Goniomenter radius
|style="background:WhiteSmoke; color:black"|
300 mm
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
300 mm
300 mm
Line 101: Line 145:
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
Minimum step size
Minimum step size
|style="background:WhiteSmoke; color:black"|
0.0001° (0.36")
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
0.0001° (0.36")
0.0001° (0.36")
Line 107: Line 153:
|-
|-
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
Sample stage
Sample stage motion
|style="background:WhiteSmoke; color:black"|
*&chi;:-5~+95°
*&phi;:0~360°
*Z:-4~+1 mm
*X,Y:&plusmn;50 mm for a 100 mm wafer
*Rx,Ry:-5~+5°
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*&chi;:-5~+95°
*&chi;:-5~+95°
Line 116: Line 168:
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
Fixed with rotation
Fixed with rotation
|-
 
|style="background:LightGrey; color:black"|
Sample size
|style="background:WhiteSmoke; color:black"|
Diameter: 150 mm
Thickness: 0~21 mm
|style="background:WhiteSmoke; color:black"|
Powders
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Optics
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Optics
Line 132: Line 177:
*In-Plane Parallel Slit Collimator (PSC)
*In-Plane Parallel Slit Collimator (PSC)
*Soller slit
*Soller slit
*Variable divergence slit
*Automatic variable divergence slit
*Length limiting slits
|style="background:WhiteSmoke; color:black"|
*Cross Beam Optics(CBO)
*Ge(400)x2 monochromator
*In-Plane Parallel Slit Collimator (PSC)
*Soller slit
*Automatic variable divergence slit
*Length limiting slits
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*0.04° soller slit
*0.04° soller slit
*Ni and Cu filter
*Ni and Cu filter
*Divergence slits
*Divergence slits
*Beam mask
*Beam masks
|-
|-
|style="background:LightGrey; color:black"|Receiver side
|style="background:LightGrey; color:black"|Receiver side
Line 145: Line 198:
*Parallel slit analysers (PSA)
*Parallel slit analysers (PSA)
*Ge(220)x2 analyser
*Ge(220)x2 analyser
|style="background:WhiteSmoke; color:black"|
*Automatic variable scattering slit
*Automatic variable receiver slit
*Parallel slit analysers (PSA)
*Ge(400)x2 analyser
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*0.04° soller slit
*0.04° soller slit
Line 151: Line 209:
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Measurement temperature
|style="background:LightGrey; color:black"|Measurement temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
Room temperature
Room temperature
Line 159: Line 219:
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
up to 150 mm wafers
up to 150 mm wafers
Thickness max 21 mm
|style="background:WhiteSmoke; color:black"|
up to 150 mm wafers
Thickness max 21 mm
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
Only for powders
Only for powders
Line 164: Line 230:
| style="background:LightGrey; color:black"|Allowed materials
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
All materials
All materials approved in the cleanroom.
 
No powders or dusty materials.
|style="background:WhiteSmoke; color:black"|
All materials have to be approved
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
All materials have to be approved
All materials have to be approved

Latest revision as of 23:02, 2 July 2025

Feedback to this page: click here

Unless otherwise stated, this page is written by DTU Nanolab internal


XRD at DTU Nanolab

We have three X-ray diffraction setups in building 346:

Experiments performed with XRD

Data analysis

For data analysis, we recommend using Rigaku SmartLab Studio for both thinfilms and basic powder analysis. If more advanced powder analysis is needed we provide access to a remote desktop with a licence for the excellent Malvern Panalytical software, HighScore.

Apart from commercial software a wide range of free software is available online for data analysis. Please let us know if you find something you'd like to recommend!

Comparison of the XRDs at Nanolab

Equipment XRD SmartLab XRD RotAnode XRD Powder
Purpose Crystal structure analysis

and thin film thickness measurement

  • Phase ID
  • Crystal Size
  • Crystallinity
  • Quality and degree of orientation
  • 3D orientation
  • Lattice strain
  • Composition
  • Twist
  • 3D lattice constant
  • Thickness
  • Roughness
  • Density
  • Phase ID
  • Crystal Size
  • Crystallinity
  • Quality and degree of orientation
  • 3D orientation
  • Lattice strain
  • Composition
  • Twist
  • 3D lattice constant
  • Thickness
  • Roughness
  • Density
  • Phase ID
  • Crystal Size
  • Crystallinity
X-ray generator

Maximum rated output

3 kW

9 kW

600 W

Rated tube voltage

20 to 45 kV

20 to 45 kV

40 kV

Rated tube current

2 to 60 mA

2 to 200 mA

15 mA

Type

Sealed tube

Rotating Anode

Sealed tube

Target

Cu

Cu

Cu

Focus size

0.4 mm x 8 mm (Line/Point)

0.1-0.5 mm x 8 mm (Line/Point)

0.4 mm x 12 mm (Line)

Goniometer

Scanning mode

incident / receiver coupled or independent

incident / receiver coupled or independent

incident / receiver coupled

Goniomenter radius

300 mm

300 mm

145 mm

Minimum step size

0.0001° (0.36")

0.0001° (0.36")

0.001° (3.6")

Sample stage motion

  • χ:-5~+95°
  • φ:0~360°
  • Z:-4~+1 mm
  • X,Y:±50 mm for a 100 mm wafer
  • Rx,Ry:-5~+5°
  • χ:-5~+95°
  • φ:0~360°
  • Z:-4~+1 mm
  • X,Y:±50 mm for a 100 mm wafer
  • Rx,Ry:-5~+5°

Fixed with rotation

Optics Incident side
  • Cross Beam Optics(CBO)
  • Ge(220)x2 monochromator
  • In-Plane Parallel Slit Collimator (PSC)
  • Soller slit
  • Automatic variable divergence slit
  • Length limiting slits
  • Cross Beam Optics(CBO)
  • Ge(400)x2 monochromator
  • In-Plane Parallel Slit Collimator (PSC)
  • Soller slit
  • Automatic variable divergence slit
  • Length limiting slits
  • 0.04° soller slit
  • Ni and Cu filter
  • Divergence slits
  • Beam masks
Receiver side
  • Automatic variable scattering slit
  • Automatic variable receiver slit
  • Parallel slit analysers (PSA)
  • Ge(220)x2 analyser
  • Automatic variable scattering slit
  • Automatic variable receiver slit
  • Parallel slit analysers (PSA)
  • Ge(400)x2 analyser
  • 0.04° soller slit
  • Ni filter
Substrates Measurement temperature

Room temperature

Room temperature

May be heated in N2 up to 500°C

Substrate size

up to 150 mm wafers

Thickness max 21 mm

up to 150 mm wafers

Thickness max 21 mm

Only for powders

Allowed materials

All materials approved in the cleanroom.

No powders or dusty materials.

All materials have to be approved

All materials have to be approved