== Silicon sputter==
{{cc-nanolab}}


Silicon can be deposited in [[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec.]]
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.labadviser.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Si_sputter_in_Wordentec click here]'''


'''<p style="color:red;">The Wordentec has been decomissioned in 2025. These results are kept for reference.</p>'''


'''Parameters'''
= Silicon sputtering in the Wordentec=


Listed below are tried parameters, that can be used during deposition.
Silicon can be sputter deposited in the [[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]] as well as in the [[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System(Lesker)]] (details on sputtering Si in the Sputter-System Lesker [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si sputter in Sputter-System Lesker|here]]) and in the new [[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Cluster Lesker]] (results [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si sputter in Sputter-System Metal-Oxide(PC1)|here]] and [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si sputter in Sputter-System Metal-Oxide(PC3)|here]]).  


==Parameters==
Listed below are tried parameters, that can be used during Si deposition in the Wordentec. The process parameters in the table below can be used as started values, run a test process to be sure that you get the right thickness.
'''Do not use the power more than 180 W without consulting staff''', since the Si target could break into a lot of small pieces.


{| border="1" cellspacing="0" cellpadding="4"  
{| border="1" cellspacing="0" cellpadding="4"  
!  
!  
! Setting
! Settings 1
! Settings 2
|-  
|-  
| Process type
| Process type
|Sputtering
|Sputtering
|Sputtering
|-  
|-  
| Power
| Power
|1000W
|130W
|-
|170W
| Base pressure
 
| 6*10<sup>-7</sup>
|-
| Ignition pressure
| 6*10<sup>-3</sup>
|-
|-
| Sputter pressure
| Sputter pressure
| 4*10<sup>-3</sup>
| 5*10<sup>-3</sup> mbar
| 1*10<sup>-2</sup> mbar
 
|-
|-
| Rate
| Rate
| About 0,14Å/s (2 wafers plates, rotating)
| About 0.7 Å/s
| About 0.6 Å/s  
|-
|-
|}
|}