Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/SiO2 Etch/Cr mask: Difference between revisions

Bghe (talk | contribs)
Mmat (talk | contribs)
mNo edit summary
 
(4 intermediate revisions by one other user not shown)
Line 4: Line 4:
=SiO2 trench etching with Cr mask=
=SiO2 trench etching with Cr mask=


[[test12]]


{| border="2" cellspacing="2" cellpadding="3"  
{| border="2" cellspacing="2" cellpadding="3"  
Line 595: Line 594:
File:C10844_13.jpg
File:C10844_13.jpg
</gallery>
</gallery>
|- style="vertical-align:top;"
|
*Coil Power [W]:300
*'''Platen Power [W]: 25'''
*Platen temperature [<sup>o</sup>C]: 20
*H2 flow [sccm]:0
*O2 flow [sccm]: 10
*C<sub>4</sub>F<sub>8</sub> flow [sccm]: 11.5
*He flow [sccm]:100
*Pressure:Fully open APC valve (<2 mTorr)
*Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
|After some major chemical cleans I could not repeat the results of C10834. I need to increase the C4F8 to fairly match the results
|
<gallery caption=" C12508: SiO2 etch with Cr mask on wafer piece on Si carrier 50 min etch, EM:0/0 H2:0sccm, C4F8:11.5sccm He:100sccm O2:10sccm, Pressure:?mTorr; platen power 25W, coil power:300W" perrow="6" widths="200px" heights="150px">
File:C12508_03__14.jpg
File:C12508_03__02.jpg
File:C12508_03__04.jpg
File:C12508_03__06.jpg
File:C12508_03__07.jpg
File:C12508_03__09.jpg
File:C12508_03__12.jpg
</gallery>
|}
|}
TEST:
[[File:C12332_06.jpg|400px]]