'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/silicon_oxide click here]''' | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/silicon_oxide click here]''' | ||
<br> | |||
It is possible to etch SiO2 in the ICP metal etcher but it is not designed for it and | =SiO2 etching in the ICP metal= | ||
It is possible to etch SiO2 in the ICP metal etcher but it is not designed for it and we prefer that you do it elsewhere. It is a challenge to get a good selectivity to resist (typically in the range of 1:1 or worse) and it is probably not possible to get a profile angle of 90 degrees. More likely about 75-85 degrees. Different chemistries can be applied either based on CF4 or C4F8. If seems that C4F8 can give the best selectivity to resist (best case I have seem was 1:11 but it depends a lot on the process parameters)). If low coil power is needed CF4 chemistry is used because C4F8 needs a higher power to generate a plasma. ''/bghe 2016-04-25 '' | |||
==Slow etch of SiO2 with resist as masking material - using a 6" carrier wafer with recess == | ==Slow etch of SiO2 with resist as masking material - using a 6" carrier wafer with recess == | ||
| Line 129: | Line 133: | ||
|Etch rate of thermal oxide | |Etch rate of thermal oxide | ||
| | | | ||
*'''145-172 nm/min''' ''by bghe@ | *'''145-172 nm/min''' ''by bghe@nanolab (2015-06-02)'' | ||
*'''145 nm/min ''' ''by Martin Lind Ommen (fall 2016)'' | *'''145 nm/min ''' ''by Martin Lind Ommen (fall 2016)'' | ||
|- | |- | ||
|Selectivity to resist [:1] | |Selectivity to resist [:1] | ||
| 4-5:1 (SiO2:resist) ''by bghe@ | | 4-5:1 (SiO2:resist) ''by bghe@nanolab (2015-06-02)'' | ||
|- | |- | ||
|Cr etch rate | |Cr etch rate | ||
| Line 139: | Line 143: | ||
|- | |- | ||
|Profile [<sup>o</sup>] | |Profile [<sup>o</sup>] | ||
|86-87 dg ''by bghe@ | |86-87 dg ''by bghe@nanolab (2015-06-02)'' | ||
|- | |- | ||
|Wafer uniformity map (click on the image to view a larger image) | |Wafer uniformity map (click on the image to view a larger image) | ||
| Line 156: | Line 160: | ||
| | | | ||
*Sample: s007592 ''by bghe@nanolab (2015-06-02)'' | *Sample: s007592 ''by bghe@nanolab (2015-06-02)'' | ||
*See Martin Lind Ommen's results with hard masks | *See Martin Lind Ommen's results with hard masks: [https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide#Dry_etch_with_Hard_mask] <br> There were problems with polymer on the surface after etching. | ||
|} | |} | ||
| Line 282: | Line 286: | ||
|-style="background:Black; color:White" | |-style="background:Black; color:White" | ||
!Results | !Results | ||
!Test on 6" wafer, by Peixiong Shi@ | !Test on 6" wafer, by Peixiong Shi@nanolab | ||
|- | |- | ||
|Etch rate of thermal oxide | |Etch rate of thermal oxide | ||