==CHF3/O2 etch== | ==CHF3/O2 etch== | ||
| Line 6: | Line 7: | ||
A plasma with a gas mixture of CHF<sub>3</sub> and O<sub>2</sub> is used to etch SiO<sub>2</sub> and Si<sub>3</sub>N<sub>4</sub> dielectricas; flour radicals are responsible for etching the dielectrica while oxygen removes the polymer that is formed during the etch. The polymer deposition rate and SiO<sub>2</sub> etch rate are very sensitive to the flow ratio of CHF<sub>3</sub> and O<sub>2</sub> . The current processes have been optimized from this point of view. | A plasma with a gas mixture of CHF<sub>3</sub> and O<sub>2</sub> is used to etch SiO<sub>2</sub> and Si<sub>3</sub>N<sub>4</sub> dielectricas; flour radicals are responsible for etching the dielectrica while oxygen removes the polymer that is formed during the etch. The polymer deposition rate and SiO<sub>2</sub> etch rate are very sensitive to the flow ratio of CHF<sub>3</sub> and O<sub>2</sub> . The current processes have been optimized from this point of view. | ||
There are | There are 4 standard programs: | ||
{| border="1" style="text-align: center; width: | {| border="1" style="text-align: center; width: 1000px; height: 350px;" | ||
! colspan=" | ! colspan="8" style="text-align: center;" style="background: #efefef;" | CHF<sub>3</sub>/O<sub>2</sub> etch rates, nm/min | ||
|- | |- | ||
! scope="row" width="15%" |Process Name | ! scope="row" width="15%" |Process Name | ||
| Line 18: | Line 19: | ||
! width="10%" |AZ5206 | ! width="10%" |AZ5206 | ||
! width="10%" |ZEP520A | ! width="10%" |ZEP520A | ||
! width="10%" |Negative DUV: UVN 2030-0.5 | |||
! width="60%" |Comments/links | |||
|- | |- | ||
!SiO2_602 | !SiO2_602 | ||
| Line 30: | Line 33: | ||
|29'''<sup>{(2)}</sup>''' | |29'''<sup>{(2)}</sup>''' | ||
|36'''<sup>{(3)}</sup>''' | |36'''<sup>{(3)}</sup>''' | ||
| | |||
| | |||
|- | |||
!High selectivity to resist | |||
! | |||
*CHF<sub>3</sub>-flow: 17 sccm, | |||
*O<sub>2</sub>-flow: 0 sccm, | |||
*Power = 150 W, | |||
*Vbias = ? V, | |||
*Process pressure = 150 mTorr | |||
|85 | |||
| | |||
| | |||
| | |||
|10.6 | |||
|[[/SiO2 DOE|Process Development]] ''dec2019/jan2020 by Qugig and bghe @nanolab'' | |||
|- | |||
!Lower etch rate, medium selectivity to resist | |||
! | |||
*CHF<sub>3</sub>-flow: 17 sccm, | |||
*O<sub>2</sub>-flow: 0 sccm, | |||
*Power = 100 W, | |||
*Vbias = ? V, | |||
*Process pressure = 20 mTorr | |||
|49-62 (depending on conditioning) | |||
| | |||
| | |||
|~12 | |||
| | |||
| [[/Details SiO2_100|Images and reproducibility]] ''dec2019/jan2020 by Qugig and bghe @nanolab'' | |||
|- | |- | ||
!Si3N4Ti | !Si3N4Ti | ||
| Line 40: | Line 73: | ||
| | | | ||
|38 | |38 | ||
| | |||
| | |||
| | | | ||
| | | | ||