Jump to content

Specific Process Knowledge/Etch/III-V RIE/III V RIE ETCHES: Difference between revisions

Bghe (talk | contribs)
Created page with "==CHF3/O2 etch== A plasma with a gas mixture of CHF<sub>3</sub> and O<sub>2</sub> is used to etch SiO<sub>2</sub> and Si<sub>3</sub>Ni<sub>4</sub> dielectricas; flour radical..."
 
Mmat (talk | contribs)
mNo edit summary
 
(20 intermediate revisions by 2 users not shown)
Line 1: Line 1:
{{cc-nanolab}}
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labnanolab.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Etch/III-V_RIE/III_V_RIE_ETCHES  click here]'''<br>
==CHF3/O2 etch==
==CHF3/O2 etch==


A plasma with a gas mixture of CHF<sub>3</sub> and O<sub>2</sub> is used to etch SiO<sub>2</sub> and Si<sub>3</sub>Ni<sub>4</sub> dielectricas; flour radicals are responsible for etching the dielectrica while oxygen removes the polymer that is formed during the etch. The polymer deposition rate and SiO<sub>2</sub>  etch rate are very sensitive to the flow ratio of CHF<sub>3</sub>  and O<sub>2</sub> . The current processes have been optimized from this point of view.
A plasma with a gas mixture of CHF<sub>3</sub> and O<sub>2</sub> is used to etch SiO<sub>2</sub> and Si<sub>3</sub>N<sub>4</sub> dielectricas; flour radicals are responsible for etching the dielectrica while oxygen removes the polymer that is formed during the etch. The polymer deposition rate and SiO<sub>2</sub>  etch rate are very sensitive to the flow ratio of CHF<sub>3</sub>  and O<sub>2</sub> . The current processes have been optimized from this point of view.


There are 3 standard programs:
There are 4 standard programs:




{| border="1" style="text-align: center; width: 600px; height: 350px;"
{| border="1" style="text-align: center; width: 1000px; height: 350px;"
! colspan="6" style="text-align: center;" style="background: #efefef;" | CHF<sub>3</sub>/O<sub>2</sub> etch rates, nm/min
! colspan="8" style="text-align: center;" style="background: #efefef;" | CHF<sub>3</sub>/O<sub>2</sub> etch rates, nm/min
|-
|-
! scope="row" width="15%" |Process Name
! scope="row" width="15%" |Process Name
Line 15: Line 19:
! width="10%" |AZ5206
! width="10%" |AZ5206
! width="10%" |ZEP520A
! width="10%" |ZEP520A
! width="10%" |Negative DUV: UVN 2030-0.5
! width="60%" |Comments/links
|-
|-
!SiO2_602  
!SiO2_602  
Line 27: Line 33:
|29'''<sup>{(2)}</sup>'''
|29'''<sup>{(2)}</sup>'''
|36'''<sup>{(3)}</sup>'''
|36'''<sup>{(3)}</sup>'''
|&nbsp;
|&nbsp;
|-
!High selectivity to resist
!
*CHF<sub>3</sub>-flow: 17 sccm,
*O<sub>2</sub>-flow: 0 sccm,
*Power = 150 W,
*Vbias = ? V,
*Process pressure = 150 mTorr
|85
|&nbsp;
|&nbsp;
|&nbsp;
|10.6
|[[/SiO2 DOE|Process Development]] ''dec2019/jan2020 by Qugig and bghe @nanolab''
|-
!Lower etch rate, medium selectivity to resist
!
*CHF<sub>3</sub>-flow: 17 sccm,
*O<sub>2</sub>-flow: 0 sccm,
*Power = 100 W,
*Vbias = ? V,
*Process pressure = 20 mTorr
|49-62 (depending on conditioning)
|&nbsp;
|&nbsp;
|~12
|&nbsp;
| [[/Details SiO2_100|Images and reproducibility]] ''dec2019/jan2020 by Qugig and bghe @nanolab''
|-
|-
!Si3N4Ti
!Si3N4Ti
Line 37: Line 73:
|&nbsp;
|&nbsp;
|38
|38
|&nbsp;
|&nbsp;
|&nbsp;
|&nbsp;
|&nbsp;
|&nbsp;
|-
|-
<!-- recipe wrong other parameters on RIE
!Si3N4Std'''<sup>{(4)}</sup>'''
!Si3N4Std'''<sup>{(4)}</sup>'''
!
!
Line 51: Line 90:
|&nbsp;
|&nbsp;
|&nbsp;
|&nbsp;
-->
|}
|}


Line 97: Line 137:
!
!
*CH<sub>4</sub>-flow: 8.4 sccm,  
*CH<sub>4</sub>-flow: 8.4 sccm,  
*H<msub>2</sub>-flow: 42 sccm,
*H<sub>2</sub>-flow: 42 sccm,
*Power = 60 W,
*Power = 60 W,
*Vbias = 450 V,
*Vbias = 450 V,
Line 114: Line 154:
There are 3 standard processes: '''BCB_LP''' and '''BCB30LP''' are low pressure (anisotropic) medium power etches for planarization of BCB, while '''BCB100W''' is a high power etch to totally remove thick layers of BCB.
There are 3 standard processes: '''BCB_LP''' and '''BCB30LP''' are low pressure (anisotropic) medium power etches for planarization of BCB, while '''BCB100W''' is a high power etch to totally remove thick layers of BCB.


Other resists (ZEP520A, AZ-resists) can be etched by a O<msub>2</sub> etch. The standard program is called '''ASH?m''', where the process time is optional.
Other resists (ZEP520A, AZ-resists) can be etched by a O<sub>2</sub> etch. The standard program is called '''ASH?m''', where the process time is optional.


{| border="1" style="text-align: center; width: 600px; height: 350px;"
{| border="1" style="text-align: center; width: 600px; height: 350px;"