Jump to content

Specific Process Knowledge/Thin film deposition/PECVD/Doping: Difference between revisions

Kabi (talk | contribs)
No edit summary
Mmat (talk | contribs)
mNo edit summary
 
(9 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/PECVD/Doping  click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/PECVD/Doping  click here]'''  


 
<span style="color:#FF0000">This work has been done on PECVD2. PECVD2 has been decomissioned but we keep this information because we expect PECVD3 and PECVD4 to behave similar</span>
 
 
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=


==Boron-doping by use of BSG glass deposited in PECVD2==
==Boron-doping by use of BSG glass deposited in PECVD2==
Line 35: Line 32:


5 tests were made where only the B<sub>2</sub>H<sub>6</sub> flow was changed for each deposition (120sccm,130sccm,140sccm,160sccm,240sccm). All deposition times were 2 min, resulting in 440 nm Oxide.
5 tests were made where only the B<sub>2</sub>H<sub>6</sub> flow was changed for each deposition (120sccm,130sccm,140sccm,160sccm,240sccm). All deposition times were 2 min, resulting in 440 nm Oxide.
The wafers were annealed in Anneal Oxide Furnace (C1) at 1000°C for 85 min to drive in the boron and the oxide was subsequently etched in BHF. The wafers were then analyzed by SIMS and the results are shown in the figure below:
The wafers were annealed in Anneal Oxide Furnace (C1) at 1000°C for 85 min to drive in the boron and the oxide was subsequently etched in BHF.  
 
The wafers were then analyzed by SIMS and the results are shown in the figure below:




Line 70: Line 69:
|}
|}


3 tests were made where only the B<sub>2</sub>H<sub>6</sub> flow was changed for each deposition (120sccm,130sccm,140sccm,160sccm,240sccm). All deposition times were 2 min, resulting in 440 nm Oxide.
3 tests were made where only the B<sub>2</sub>H<sub>6</sub> flow was changed for each deposition (120sccm,130sccm,140sccm,160sccm,240sccm). All deposition times were 2 min, resulting in approximately 400nm Oxide.
 
The wafers were going through several annealing and oxidation step:
The wafers were going through several annealing and oxidation step:


Line 84: Line 84:


[[image:PECVD_Boron_doping_profiles.jpg|627x424px|left|thumb|Boron concentration measured by SIMS. Results from Trine Holm Christensen, Space, Feb. 2015.]]
[[image:PECVD_Boron_doping_profiles.jpg|627x424px|left|thumb|Boron concentration measured by SIMS. Results from Trine Holm Christensen, Space, Feb. 2015.]]
<br clear="all" />
Measured peak concentrations and sheet resistances:
<br>
{| border="1" cellspacing="0" cellpadding="7" with="50" style="text-align:center;"
|-
|Wafer
|Peak Concentration
[atoms/cm<sup>3</sup>]
|Sheet Resistance
[&Omega;/sq]
|-
|BSG120
|1.75*10<sup>19</sup>
|56.4
|-
|BSG130
|2.44*10<sup>19</sup>
|36.2
|-
|BSG140
|2.36*10<sup>19</sup>
|40.3
|-
|}