Jump to content

Specific Process Knowledge/Back-end processing/Polisher CMP: Difference between revisions

From LabAdviser
Rkch (talk | contribs)
Mmat (talk | contribs)
mNo edit summary
 
(14 intermediate revisions by 3 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Back-end_processing/Polisher_CMP click here]'''
{{cc-nanolab}}
 
 




'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Back-end_processing/Polisher_CMP click here]'''
<br>
<br>
== Polisher (CMP) ==
== Polisher (CMP) ==


[[image:Cmp_picture.jpg|400px|right|thumb|The Logitech PM5 Polisher/Lapper]]
[[image:Cmp_picture.jpg|400px|right|thumb|The Logitech PM5 Polisher/Lapper in cleanroom A-5]]


The Logitech Orbis Polisher (CMP) is for polishing wafers (removing material in the nm range) it is not for thinning down wafers or other substrates.
The Logitech Orbis Polisher (CMP) is for polishing wafers (removing material in the nm range) it is not for thinning down wafers or other substrates. After CMP it is recommended to use the '''[http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Wafer_cleaning/Post_CMP_Cleaner Post CMP Cleaner]''' to clean the sample for slurry residues left by the CMP.




Line 16: Line 17:
<!-- give the link to the equipment info page in LabManager: -->
<!-- give the link to the equipment info page in LabManager: -->
[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=430 The Logitech Orbis (CMP) in LabManager]
[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=430 The Logitech Orbis (CMP) in LabManager]


==Equipment performance and process related parameters==
==Equipment performance and process related parameters==
Line 28: Line 28:
!style="background:silver; color:black;" align="center" width="60"|Purpose  
!style="background:silver; color:black;" align="center" width="60"|Purpose  
|style="background:LightGrey; color:black"|  
|style="background:LightGrey; color:black"|  
Thinning of substrates of
Polishing of
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*InP
*GaAs
*Silicon
*Silicon
*Metals
*SiO2
*Glass/Quartz
<!-- |style="background:WhiteSmoke; color:black"|
<!-- |style="background:WhiteSmoke; color:black"|
*Purpose 1
*Purpose 1
Line 41: Line 38:
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Performance
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Performance
|style="background:LightGrey; color:black"| Thinning
|style="background:LightGrey; color:black"| 20x20mm substrate
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Removal rate: 1-10µm/min
*Removal rate: 400nm/min
*Thickness accuracy: +/- 10 µm
*Thickness accuracy: +/- ? µm
*Thickness homogeneity: +/- 10 µm
*Thickness homogeneity: +/- ? µm
*Roughness: +/- ? µm
*Roughness: +/- ? µm
<!-- |style="background:WhiteSmoke; color:black"|
<!-- |style="background:WhiteSmoke; color:black"|
Line 52: Line 49:
*Performance range 3 -->
*Performance range 3 -->
|-
|-
|style="background:LightGrey; color:black"|Polishing
|style="background:LightGrey; color:black"|100mm substrate
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Removal rate: ~1 µm/min
*Removal rate: ~ 60 nm/min
*Thickness accuracy: ? µm
*Thickness accuracy: ? µm
*Thickness homogeneity: ? µm
*Thickness homogeneity: ? µm
Line 64: Line 61:
|style="background:LightGrey; color:black"|Polishing liquid
|style="background:LightGrey; color:black"|Polishing liquid
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Al2O3 (alumina) powder: 3, 9 or 20 µm
*SF1 Polishing Fluid
*Chemlox (for polishing)
*SF1 Polishing Fluid (for polishing e.g. SiO2)
|-
|-
|style="background:LightGrey; color:black"|Polishing cloths
|style="background:LightGrey; color:black"|Polishing cloths
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Chemcloth Polishing Cloths (for use with SF1 liquid)
*Chemcloth Polishing Cloths
|-
|-
|style="background:LightGrey; color:black"|Rotation speed
|style="background:LightGrey; color:black"|Rotation
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Thinning: 5-20 rpm
*Plate
*Polishing: 5-80 rpm
*Head/Puck
|-
|-
|style="background:LightGrey; color:black"|Arm sweep
|style="background:LightGrey; color:black"|Arm sweep
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Thinning: stationary
*Polishing: 20% (inner) - 100% (outer)
*Polishing: 12% (inner) - 80% (outer)
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Batch size
|style="background:LightGrey; color:black"|Sample size
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*<nowiki>#</nowiki> small samples
*<nowiki></nowiki> one 20x20mm piece
*one 50 mm wafer
*one 50 mm wafer
*one 2" wafer
*one 100 mm wafer
*one 100 mm wafer
*one 150 mm wafer
<!-- |style="background:WhiteSmoke; color:black"|
<!-- |style="background:WhiteSmoke; color:black"|
*<nowiki>#</nowiki> small samples
*<nowiki>#</nowiki> small samples
Line 96: Line 92:
| style="background:LightGrey; color:black"|Allowed materials
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*InP
*GaAs
*Silicon
*Silicon
*Metals
*Glass/Quartz
*Glass/Quartz
<!-- |style="background:WhiteSmoke; color:black"|
<!-- |style="background:WhiteSmoke; color:black"|

Latest revision as of 19:06, 27 May 2025

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.


Feedback to this page: click here

Polisher (CMP)

The Logitech PM5 Polisher/Lapper in cleanroom A-5

The Logitech Orbis Polisher (CMP) is for polishing wafers (removing material in the nm range) it is not for thinning down wafers or other substrates. After CMP it is recommended to use the Post CMP Cleaner to clean the sample for slurry residues left by the CMP.


The user manual, user APV, technical information and contact information can be found in LabManager:

The Logitech Orbis (CMP) in LabManager

Equipment performance and process related parameters

Equipment Polisher/Lapper
Purpose

Polishing of

  • Silicon
  • SiO2
Performance 20x20mm substrate
  • Removal rate: 400nm/min
  • Thickness accuracy: +/- ? µm
  • Thickness homogeneity: +/- ? µm
  • Roughness: +/- ? µm
100mm substrate
  • Removal rate: ~ 60 nm/min
  • Thickness accuracy: ? µm
  • Thickness homogeneity: ? µm
  • Roughness: +/- ? µm
Process parameter range Polishing liquid
  • SF1 Polishing Fluid
Polishing cloths
  • Chemcloth Polishing Cloths
Rotation
  • Plate
  • Head/Puck
Arm sweep
  • Polishing: 20% (inner) - 100% (outer)
Substrates Sample size
  • one 20x20mm piece
  • one 50 mm wafer
  • one 2" wafer
  • one 100 mm wafer
  • one 150 mm wafer
Allowed materials
  • Silicon
  • Glass/Quartz