<!--Checked for updates on 4/4-2025 - ok/jmli --> | |||
== The Sinano3.4 recipe == | == The Sinano3.4 recipe == | ||
<!-- revised 1/6-2015 by jmli --> | |||
{| border="2" cellpadding="2" cellspacing="1" | {| border="2" cellpadding="2" cellspacing="1" | ||
|+ '''Recipe Sinano3.4''' | |+ '''Recipe Sinano3.4''' | ||
| Line 31: | Line 36: | ||
|- | |- | ||
| Mask | | Mask | ||
| 180 nm zep etched down to 72 nm | | The [[Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/nanoetch/180nmzep|180 nm zep resist]] etched down to 72 nm | ||
|- | |- | ||
|} | |} | ||
Latest revision as of 08:36, 4 April 2025
The Sinano3.4 recipe
| Recipe | Gas | BCl3 5 sccm, HBR 15 sccm |
|---|---|---|
| Pressure | 2 mTorr, Strike 3 secs @ 5 mTorr | |
| Power | 900 W CP, 90 W PP | |
| Temperature | 20 degs | |
| Hardware | 100 mm Spacers | |
| Time | 120 secs | |
| Conditions | Run ID | 431 ID |
| Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | |
| Mask | The 180 nm zep resist etched down to 72 nm |
- The results of the Sinano3.4 recipe
-
The 30 nm trenches
-
The 60 nm trenches
-
The 90 nm trenches
-
The 120 nm trenches
-
The 150 nm trenches
| Nominal trench line width | ' | ' | 30 | 60 | 90 | 120 | 150 | Average | Std. dev. |
| Etch rate | nm/min | 78 | 114 | 125 | 129 | 133 | 116 | 22 | |
| Sidewall angle | degs | 83,07278187 | 82,82949277 | 81,35457747 | 80,01059257 | 80,6398092 | 82 | 1 | |
| CD loss | nm/edge | -13 | -11 | -12 | -12 | -5 | -11 | 3 | |
| CD loss foot | nm/edge | -13 | -2 | 3 | 6 | 15 | 2 | 10 | |
| Bowing | 9 | 8 | 6 | 6 | -1 | 5 | 4 | ||
| Bottom curvature | -22 | -10 | -6 | -4 | -6 | -9 | 7 | ||
| Zep etch rate | 67 |