Jump to content

Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/Sinano36: Difference between revisions

From LabAdviser
Jml (talk | contribs)
Created page with "== The Sinano3.6 recipe == {| border="2" cellpadding="2" cellspacing="1" |+ '''Recipe Sinano3.6''' |- ! rowspan="6" align="center"| Recipe | Gas | BCl<sub>3</sub> 5 sccm, HB..."
 
Jmli (talk | contribs)
No edit summary
 
(4 intermediate revisions by the same user not shown)
Line 1: Line 1:
<!--Checked for updates on 10/7-2019 - ok/jmli -->
<!-- Ok, jmli 20170627 -->
<!--Checked for updates on 24/8-2021. ok/ jmli-->
<!--Checked for updates on 4/4-2025 - ok/jmli -->
== The Sinano3.6 recipe ==
== The Sinano3.6 recipe ==
 
<!-- revised 1/6-2015 by jmli -->
{| border="2" cellpadding="2" cellspacing="1"  
{| border="2" cellpadding="2" cellspacing="1"  
|+ '''Recipe Sinano3.6'''
|+ '''Recipe Sinano3.6'''

Latest revision as of 08:34, 4 April 2025


The Sinano3.6 recipe

Recipe Sinano3.6
Recipe Gas BCl3 5 sccm, HBR 15 sccm
Pressure 10 mTorr, Strike 3 secs @ 5 mTorr
Power 900 W CP, 60 W PP
Temperature 20 degs
Hardware 100 mm Spacers
Time 180 secs
Conditions Run ID 441, 442 ID
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask 190 nm zep etched down to 56 nm


Nominal trench line width ' ' 30 60 90 120 150 Average Std. dev.
Etch rate nm/min 24 85 94 94 96 79 31
Sidewall angle degs 80 83 83 83 83 83 2
CD loss nm/edge -22 -23 -34 -35 -31 -29 6
CD loss foot nm/edge -22 -14 -19 -17 -11 -17 4
Bowing 5 13 21 21 17 15 6
Bottom curvature -30 -14 -9 6 5 -8 15
Zep etch rate 45