Specific Process Knowledge/Wafer cleaning/Cleaning with Soap Sonic: Difference between revisions
| (23 intermediate revisions by 4 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:wetchemistry@ | '''Feedback to this page''': '''[mailto:wetchemistry@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Wafer_cleaning/Cleaning_with_Soap_Sonic click here]''' | ||
== | '''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.''' | ||
'''All links to Labmanager requires login.''' | |||
=Bringing samples into the DTU Nanolab cleanroom= | |||
To avoid cross contamination of fabrication tools and in order to keep particle levels at a minimum it is in general not allowed to bring substrates processed outside the cleanroom into the cleanroom. Users who need to bring this type of substrates into the cleanroom for processing or characterization must obtain permission to do so. This can be obtained by filling out the [[:File:Request to bring Samples into CR v1.51.docx|Request to bring samples into cleanroom form]] and submitting it to [mailto:training@nanolab.dtu.dk training@nanolab.dtu.dk]. | |||
If permission is granted the standard cleaning process for the approved substrates are | |||
# Triton-X soap cleaning as described below | |||
# 10 min cleaning in a piranha solution (sulphuric acid and hydrogen peroxide) | |||
If the samples can not handle such a cleaning process it must be specified in the form and an alternative cleaning process must be suggested by the user. | |||
==Triton-X soap cleaning== | |||
[[Image:Sonic-clean.jpg|300x300px|thumb|Soap sonic clean placed in the wash bench in the changing room (gowning). ]] | [[Image:Sonic-clean.jpg|300x300px|thumb|Soap sonic clean placed in the wash bench in the changing room (gowning). ]] | ||
The soap sonic is done in a tank with ultrasonics placed in the cleaning bench in the changing room. The cleaning solution is DI water to which a little diluted Triton X-100 is added. Triton X-100 is a nonionic detergent which is free | The soap sonic is done in a tank with ultrasonics placed in the cleaning bench in the changing room. The cleaning solution is DI water to which a little diluted Triton X-100 is added. Triton X-100 is a nonionic detergent which is metal ion free. This detergent is added to reduce surface tension and thus help removing particles from the samples to be cleaned. | ||
===Procedure=== | ===Procedure=== | ||
The bench in gowning contains a sink, an ultrasonics bath and a rinse bath for rinsing samples cleaned in Triton X-100. To clean the samples: | |||
*Fill | *Find a suitable holder for your samples in the cupboard below the baths | ||
*Make sure the ultrasonics bath dump valve is closed | |||
*Fill the ultrasonics bath (the one made of metal) with DI water (enough to completely cover your samples) | |||
*Add 20 - 30 drops of diluted Triton X-100 detergent (From the rinse/spray bottle. Do '''''NOT''''' use undiluted Triton X-100) | *Add 20 - 30 drops of diluted Triton X-100 detergent (From the rinse/spray bottle. Do '''''NOT''''' use undiluted Triton X-100) | ||
*Start ultrasonics | *Close the bath lid to minimize noise from the ultrasonics bath | ||
*Start ultrasonics on the front panel | |||
*Leave sample in ultrasonics for 10 min | *Leave sample in ultrasonics for 10 min | ||
*Switch off ultrasonics | *Switch off ultrasonics | ||
*Fill rinse bath with DI water and rinse samples | *Fill rinse bath (the one made in plastic) with DI water and rinse your samples | ||
*Remove samples and dry them | *Remove samples and dry them | ||
*Dump the Triton X-100 and rinse | *Dump the Triton X-100 solution and rinse baths to drain. Rinse tanks with DI water. Leave dump valves open so the baths drain completely | ||
*Continue with piranha. | *Continue with [http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Wafer_cleaning/7-up_%26_Piranha piranha]. | ||
Latest revision as of 09:20, 1 April 2025
Feedback to this page: click here
Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.
All links to Labmanager requires login.
Bringing samples into the DTU Nanolab cleanroom
To avoid cross contamination of fabrication tools and in order to keep particle levels at a minimum it is in general not allowed to bring substrates processed outside the cleanroom into the cleanroom. Users who need to bring this type of substrates into the cleanroom for processing or characterization must obtain permission to do so. This can be obtained by filling out the Request to bring samples into cleanroom form and submitting it to training@nanolab.dtu.dk.
If permission is granted the standard cleaning process for the approved substrates are
- Triton-X soap cleaning as described below
- 10 min cleaning in a piranha solution (sulphuric acid and hydrogen peroxide)
If the samples can not handle such a cleaning process it must be specified in the form and an alternative cleaning process must be suggested by the user.
Triton-X soap cleaning

The soap sonic is done in a tank with ultrasonics placed in the cleaning bench in the changing room. The cleaning solution is DI water to which a little diluted Triton X-100 is added. Triton X-100 is a nonionic detergent which is metal ion free. This detergent is added to reduce surface tension and thus help removing particles from the samples to be cleaned.
Procedure
The bench in gowning contains a sink, an ultrasonics bath and a rinse bath for rinsing samples cleaned in Triton X-100. To clean the samples:
- Find a suitable holder for your samples in the cupboard below the baths
- Make sure the ultrasonics bath dump valve is closed
- Fill the ultrasonics bath (the one made of metal) with DI water (enough to completely cover your samples)
- Add 20 - 30 drops of diluted Triton X-100 detergent (From the rinse/spray bottle. Do NOT use undiluted Triton X-100)
- Close the bath lid to minimize noise from the ultrasonics bath
- Start ultrasonics on the front panel
- Leave sample in ultrasonics for 10 min
- Switch off ultrasonics
- Fill rinse bath (the one made in plastic) with DI water and rinse your samples
- Remove samples and dry them
- Dump the Triton X-100 solution and rinse baths to drain. Rinse tanks with DI water. Leave dump valves open so the baths drain completely
- Continue with piranha.