'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.''' | |||
'''All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.''' | |||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Gold click here]''' | |||
'''Feedback to this page''': '''[mailto:labadviser@ | |||
==Etching of Gold== | ==Etching of Gold== | ||
Etching of Gold can be done either by wet etch, | Etching of Gold can be done either by wet etch, or by sputtering with ions. | ||
*[[Specific Process Knowledge/Etch/Wet Gold Etch|Etching of Gold by wet etch]] | *[[Specific Process Knowledge/Etch/Wet Gold Etch|Etching of Gold by wet etch]] | ||
*[[Specific_Process_Knowledge/Etch/IBE⁄IBSD Ionfab 300/IBE Au etch|Sputtering of Au]] | *[[Specific_Process_Knowledge/Etch/IBE⁄IBSD Ionfab 300/IBE Au etch|Sputtering of Au]] | ||
| Line 81: | Line 20: | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
! | ! | ||
![[Specific Process Knowledge/Etch/Wet | ![[Specific Process Knowledge/Etch/Wet Gold Etch|Au wet etch 1]] | ||
![[Specific Process Knowledge/Etch/Wet | ![[Specific Process Knowledge/Etch/Wet Gold Etch|Au wet etch 2]] | ||
![[Specific_Process_Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE (Ionfab300+)]] | ![[Specific_Process_Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE (Ionfab300+)]] | ||
|- | |- | ||
| Line 89: | Line 28: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!Generel description | !Generel description | ||
|Wet etch of | |Wet etch of Au using iodine based chemistry | ||
|Wet etch of | |Wet etch of Au using Aqua Regina | ||
|Sputtering of | |Sputtering of Au - pure physical etch | ||
|- | |- | ||
| Line 98: | Line 37: | ||
!Etch rate range | !Etch rate range | ||
| | | | ||
*~100nm/min | *~100nm/min | ||
| | | | ||
* | *680 nm/min (dilute) or faster (concentrated). Mainly used for complete removal of metals | ||
| | | | ||
*~ | *~55nm/min (acceptance test) | ||
|- | |- | ||
| Line 114: | Line 53: | ||
| | | | ||
*Anisotropic (angles sidewalls, typical around 70 dg) | *Anisotropic (angles sidewalls, typical around 70 dg) | ||
|- | |||
|-style="background:LightGrey; color:black" | |||
!Masking material | |||
| | |||
*Photoresist | |||
| | |||
*None (mainly used for stripping Au) | |||
| | |||
*Any material that is allowed in the chamber, photoresists included | |||
|- | |- | ||
|- | |- | ||
|-style="background: | |-style="background:WhiteSmoke; color:black" | ||
!Substrate size | !Substrate size | ||
| | | | ||
* | *Any size and number that can go inside the beaker in use | ||
| | | | ||
* | *Any size and number that can go inside the beaker in use | ||
| | | | ||
Smaller pieces glued to carrier wafer | Smaller pieces glued to carrier wafer | ||
| Line 133: | Line 83: | ||
|- | |- | ||
|-style="background: | |-style="background:LightGrey; color:black" | ||
!'''Allowed materials''' | !'''Allowed materials''' | ||
| | | | ||
No restrictions cross contamination wise as long as you use the right beaker and make sure that they are safe to enter in the chemicals | |||
| | | | ||
No restrictions cross contamination wise as long as you use the right beaker and make sure that they are safe to enter in the chemicals | |||
| | | | ||
*Silicon | *Silicon | ||