Specific Process Knowledge/Etch/Etching of Silicon Nitride: Difference between revisions
Appearance
| (54 intermediate revisions by 8 users not shown) | |||
| Line 1: | Line 1: | ||
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.''' | |||
'''All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.''' | |||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Silicon_Nitride click here]''' | |||
'''Feedback to this page''': '''[mailto:labadviser@ | |||
<!-- Replace "http://labadviser.danchip.dtu.dk/..." with the link to the Labadviser page--> | <!-- Replace "http://labadviser.danchip.dtu.dk/..." with the link to the Labadviser page--> | ||
== Comparing silicon etch | == Comparing silicon nitride etch methods at DTU Nanolab == | ||
There are a broad | There are a broad variety of silicon nitride etch methods at DTU Nanolab. The methods are compared here to make it easier for you to compare and choose the one that suits your needs. | ||
*[[Specific Process Knowledge/Etch/Wet Silicon Nitride Etch|Wet Silicon Nitride Etch]] | *[[Specific Process Knowledge/Etch/Wet Silicon Nitride Etch|Wet Silicon Nitride Etch]] | ||
*[[Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)/Silicon Nitride Etch using AOE|Etch of Silicon Nitride using AOE]] | *[[Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)/Silicon Nitride Etch using AOE|Etch of Silicon Nitride using AOE]] | ||
*[[Specific Process Knowledge/Etch/IBE | *[[Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide/SiO2_etch_using_ASE|Nitride etch using ASE]] | ||
*[[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE/Ion Beam Etching using IBSD Ionfab 300]] | |||
==Compare the | *[[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/silicon_nitride|Silicon nitride etch using the ICP metal]] | ||
==Compare the methods for Silicon Nitride etching== | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | ||
| Line 114: | Line 26: | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
! | ! | ||
![[Specific Process Knowledge/Etch/ | ![[Specific Process Knowledge/Etch/Wet Silicon Nitride Etch|Wet Silicon Nitride Etch]] | ||
![[Specific Process Knowledge/Etch/Wet | ![[Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF)|BHF]] | ||
![[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-4|Pegasus 4]] | |||
![[ | ![[Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)|AOE (Advanced Oxide Etch)]] | ||
![[Specific Process Knowledge/Etch/ | ![[Specific Process Knowledge/Etch/ASE_(Advanced_Silicon_Etch)|ASE]] | ||
![[Specific Process Knowledge/Etch/ | |||
![[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE/IBSD Ionfab 300]] | ![[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE/IBSD Ionfab 300]] | ||
![[Specific Process Knowledge/Etch/ICP Metal Etcher|ICP Metal]] | |||
|- | |- | ||
| Line 128: | Line 41: | ||
!Generel description | !Generel description | ||
| | | | ||
* | *Isotropic etch | ||
*Well suited for removing all nitride on a wafer surface (nitride strip) without a mask. High selectivity Si<sub>3</sub>N<sub>4</sub>/Si (>100) and Si<sub>3</sub>N<sub>4</sub>/SiO<sub>2</sub> (>20) @ 160 C. | |||
| | | | ||
*Isotropic etch | *Isotropic etch | ||
*Well suited for removing all PECVD nitride on a wafer surface (nitride strip) without a mask. Etches LPCVD nitride very slowly | |||
| | | | ||
* | |||
* Anisotropic etch: vertical sidewalls | |||
* With cassette loader for batch processing. | |||
| | | | ||
* | *Anisotropic etch: vertical sidewalls | ||
* | *Deep etch | ||
| | | | ||
* | *Anisotropic etch: vertical sidewalls | ||
* | *Primarily for samples with small amounts of metal | ||
| | | | ||
* | *Primarily for pure physical etch by sputtering with Ar-ions | ||
| | | | ||
*Primarily for | *Anisotropic etch: vertical sidewalls | ||
*Primarily for Cl/Br etch chemistry. | |||
*F-chemistry, please use AOE or Pegasus 4. | |||
|- | |- | ||
| Line 152: | Line 68: | ||
!Possible masking materials | !Possible masking materials | ||
| | | | ||
*Silicon Oxide | *Silicon Oxide | ||
*PolySilicon | |||
| | | | ||
*Photoresist | *Photoresist | ||
*PolySilicon | |||
*Blue film | |||
| | | | ||
*Photoresist | *Photoresist | ||
*DUV resist | |||
*E-beam resist | *E-beam resist | ||
*Silicon Oxide | *Silicon Oxide | ||
*Silicon Nitride | *Silicon Nitride | ||
*Aluminium | *Aluminium | ||
*Chromium ( | *Chromium (if needed) | ||
| | | | ||
*Photoresist | *Photoresist | ||
*DUV resist | |||
*E-beam resist | |||
*Silicon Oxide | *Silicon Oxide | ||
*Silicon Nitride | *Silicon Nitride | ||
*Aluminium | *Aluminium | ||
*Chromium (if needed) | |||
| | | | ||
* | *Photoresist | ||
*DUV resist | |||
*E-beam resist | |||
*Silicon Oxide | *Silicon Oxide | ||
*Silicon Nitride | *Silicon Nitride | ||
*Aluminium | *Aluminium | ||
* | *Metals if they cover less than 5% of the wafer area | ||
| | | | ||
*Any material that is accepted in the machine | *Any material that is accepted in the machine | ||
| | |||
*Resists | |||
*other materials from the allowed list of materials | |||
|- | |- | ||
| Line 189: | Line 109: | ||
!Etch rate range | !Etch rate range | ||
| | | | ||
*Si | *Si<sub>3</sub>N<sub>4</sub> @ 160 <sup>o</sup>C: ~26 Å/min | ||
| | | | ||
*~100- | *PECVD nitride: ~40.0-100.0 nm/min | ||
*Stoichiometric LPCVD nitride: ~0.65-8 nm/min <!-- Copyrigth issues kabi (''Yannick Seis, KU, 2019'')--> | |||
| | | | ||
* | *Process dependent. | ||
*From 0 to ~300 nm/min | |||
| | | | ||
* | *Process dependent. | ||
*from 0 to ~500 nm/min | |||
| | | | ||
* | *Probably between 20-300 nm/min depending on the process parameters | ||
| | | | ||
*Process | *Process dependent. | ||
*Has not been tested yet. | |||
| | | | ||
*Process | *Process dependent | ||
*60-65 nm/min has been tested | |||
|- | |- | ||
| Line 210: | Line 133: | ||
!Substrate size | !Substrate size | ||
| | | | ||
*<nowiki>#</nowiki>1-25 4" and 6" wafers | |||
*<nowiki>#</nowiki>1- | |||
| | | | ||
*<nowiki>#</nowiki>25 | *<nowiki>#</nowiki>1-25 4"-6" wafers | ||
| | | | ||
*As many small samples as can be | *As many small samples as can be bonded on a 150mm wafer | ||
*<nowiki>#</nowiki>1 | *50 mm wafers if bonded on a 150mm wafer | ||
* | *<nowiki>#</nowiki>1 100 mm wafer if bonded on a 150 mm wafer | ||
*#1 150 mm wafer | |||
| | | | ||
*As many small samples as can be fitted on a 100mm wafer | *As many small samples as can be fitted on a 100mm wafer | ||
*<nowiki>#</nowiki>1 50 mm wafer fitted on a 100mm wafer | *<nowiki>#</nowiki>1 50 mm wafer fitted on a 100mm wafer | ||
*<nowiki>#</nowiki>1 100 mm wafer | *<nowiki>#</nowiki>1 100 mm wafer | ||
| | | | ||
*As many small samples as can be fitted on | *As many small samples as can be fitted on the 100mm carrier (bad/no cooling!) | ||
*<nowiki>#</nowiki>1 | *<nowiki>#</nowiki>1 100mm wafer (or smaller with carrier) | ||
*<nowiki>#</nowiki>1 | *<nowiki>#</nowiki>1 150mm wafer (only when the system is set up for 150mm) | ||
| | | | ||
*As many samples as can be securely fitted on a up to 200mm wafer | *As many samples as can be securely fitted on a up to 200mm wafer | ||
| Line 240: | Line 155: | ||
*<nowiki>#</nowiki>1 150 mm wafers with special carrier | *<nowiki>#</nowiki>1 150 mm wafers with special carrier | ||
*<nowiki>#</nowiki>1 200 mm wafer | *<nowiki>#</nowiki>1 200 mm wafer | ||
| | |||
*Set up for 150mm wafers | |||
*Smaller samples can be processes when fixed to a 150mm carrier wafer. | |||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
| Line 248: | Line 166: | ||
*Silicon Nitride | *Silicon Nitride | ||
*Silicon Oxynitride | *Silicon Oxynitride | ||
| | | | ||
*Silicon | *Silicon | ||
| Line 255: | Line 172: | ||
*Silicon Oxynitride | *Silicon Oxynitride | ||
*Photoresist | *Photoresist | ||
*Blue film | |||
| | | | ||
*Silicon | *Silicon | ||
| Line 261: | Line 179: | ||
*Silicon Oxynitride | *Silicon Oxynitride | ||
*Photoresist | *Photoresist | ||
*E-beam | *E-beam resists | ||
* | *DUV resists | ||
*Aluminium (only for masking | |||
*Chromium (only for masking and on the back side if fused silica) | |||
*Quartz/fused silica | *Quartz/fused silica | ||
| | | | ||
| Line 270: | Line 190: | ||
*Silicon Oxynitride | *Silicon Oxynitride | ||
*Photoresist | *Photoresist | ||
* | *E-beam resists | ||
*Aluminium | *DUV resists | ||
*Aluminium | |||
*Chromium (only for masking and on the back side if fused silica) | |||
*Quartz/fused silica | *Quartz/fused silica | ||
| | | | ||
| Line 279: | Line 201: | ||
*Silicon Oxynitride | *Silicon Oxynitride | ||
*Photoresist | *Photoresist | ||
*E-beam | *E-beam resists | ||
* | *DUV resists | ||
* | *Other metals if they cover less than 5% of the wafer area | ||
*Quartz/fused silica | *Quartz/fused silica | ||
| | | | ||
| Line 305: | Line 218: | ||
*Polymers | *Polymers | ||
*Capton tape | *Capton tape | ||
| | |||
*Silicon | |||
*Silicon Oxide | |||
*Silicon Nitride | |||
*Silicon Oxynitride | |||
*Photoresist | |||
*E-beam resists | |||
*DUV resists | |||
*Aluminium (Al, Al2O3, AlN) | |||
*Chromium | |||
*Titanium (Ti, TiW, TiN, TiO2) | |||
*Tungsten (W) | |||
*Molybdynem | |||
*Quartz/fused silica | |||
|- | |- | ||
|} | |} | ||
<br clear="all" /> | <br clear="all" /> | ||
Latest revision as of 09:46, 26 March 2025
Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.
All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.
Feedback to this page: click here
Comparing silicon nitride etch methods at DTU Nanolab
There are a broad variety of silicon nitride etch methods at DTU Nanolab. The methods are compared here to make it easier for you to compare and choose the one that suits your needs.
- Wet Silicon Nitride Etch
- Etch of Silicon Nitride using AOE
- Nitride etch using ASE
- IBE/Ion Beam Etching using IBSD Ionfab 300
Compare the methods for Silicon Nitride etching
| Wet Silicon Nitride Etch | BHF | Pegasus 4 | AOE (Advanced Oxide Etch) | ASE | IBE/IBSD Ionfab 300 | ICP Metal
| |
|---|---|---|---|---|---|---|---|
| Generel description |
|
|
|
|
|
|
|
| Possible masking materials |
|
|
|
|
|
|
|
| Etch rate range |
|
|
|
|
|
|
|
| Substrate size |
|
|
|
|
|
|
|
| Allowed materials |
|
|
|
|
|
|
|