Silicon nitride can be etched using either wet chemistry or dry etch equipment. Wet chemistry is mainly used to remove all the nitride on the surface (backside and frontside) of a wafer. Dry etching etches one side at a time and can be used to etch structures with several masking materials.
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''
 
'''All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.'''
 
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Silicon_Nitride click here]'''
<!-- Replace "http://labadviser.danchip.dtu.dk/..." with the link to the Labadviser page-->
 
== Comparing silicon nitride etch methods at DTU Nanolab ==
 
There are a broad variety of silicon nitride etch methods at DTU Nanolab. The methods are compared here to make it easier for you to compare and choose the one that suits your needs.  
 


*[[Specific Process Knowledge/Etch/Wet Silicon Nitride Etch|Wet Silicon Nitride Etch]]
*[[Specific Process Knowledge/Etch/Wet Silicon Nitride Etch|Wet Silicon Nitride Etch]]
*[[/Etch of Silicon Nitride using RIE|Etch of Silicon Nitride using RIE]]
*[[Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)/Silicon Nitride Etch using AOE|Etch of Silicon Nitride using AOE]]
*[[Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide/SiO2_etch_using_ASE|Nitride etch using ASE]]
*[[Specific Process Knowledge/Etch/IBE&frasl;IBSD Ionfab 300|IBE/Ion Beam Etching using IBSD Ionfab 300]]
 
*[[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/silicon_nitride|Silicon nitride etch using the ICP metal]]
 
==Compare the methods for Silicon Nitride etching==
 
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"
|-
 
|-
|-style="background:silver; color:black"
!
![[Specific Process Knowledge/Etch/Wet Silicon Nitride Etch|Wet Silicon Nitride Etch]]
![[Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF)|BHF]]
![[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-4|Pegasus 4]]
![[Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)|AOE (Advanced Oxide Etch)]]
![[Specific Process Knowledge/Etch/ASE_(Advanced_Silicon_Etch)|ASE]]
![[Specific Process Knowledge/Etch/IBE&frasl;IBSD Ionfab 300|IBE/IBSD Ionfab 300]]
![[Specific Process Knowledge/Etch/ICP Metal Etcher|ICP Metal]]


==Comparison of wet Silicon Nitride etch and RIE etch for etching of Silicon Nitride==
 
{| border="2" cellspacing="0" cellpadding="4" align="center"
|-
!
 
! Wet Silicon Nitride etch
|-
! Buffered HF (BHF)
|-style="background:WhiteSmoke; color:black"
! RIE
!Generel description
|- valign="top"
! General description
|
|
*Isotropic etch
*Isotropic etch
*Well suited for removing all nitride on a wafer surface (nitride strip) without a mask. High selectivity Si<sub>3</sub>N<sub>4</sub>/Si (>100) and Si<sub>3</sub>N<sub>4</sub>/SiO<sub>2</sub> (>20) @ 180 C.
*Well suited for removing all nitride on a wafer surface (nitride strip) without a mask. High selectivity Si<sub>3</sub>N<sub>4</sub>/Si (>100) and Si<sub>3</sub>N<sub>4</sub>/SiO<sub>2</sub> (>20) @ 160 C.
|  
|
*Isotropic etch
*Isotropic etch
*Well suited for removing all  PECVD nitride on a wafer surface (nitride strip) without a mask. Etches LPCVD nitride very slowly
*Well suited for removing all  PECVD nitride on a wafer surface (nitride strip) without a mask. Etches LPCVD nitride very slowly
|  
|
 
* Anisotropic etch: vertical sidewalls
* With cassette loader for batch processing.
|
*Anisotropic etch: vertical sidewalls
*Anisotropic etch: vertical sidewalls
|- valign="top"
*Deep etch
!Possible masking materials:
|
*Anisotropic etch: vertical sidewalls
*Primarily for samples with small amounts of metal
|
*Primarily for pure physical etch by sputtering with Ar-ions
|
*Anisotropic etch: vertical sidewalls
*Primarily for Cl/Br etch chemistry.
*F-chemistry, please use AOE or Pegasus 4.
|-
 
|-
|-style="background:LightGrey; color:black"
!Possible masking materials
|
|
*Silicon Oxide
*Silicon Oxide
Line 31: Line 76:
|
|
*Photoresist
*Photoresist
*DUV resist
*E-beam resist
*Silicon Oxide
*Silicon Oxide
*Silicon Nitride
*Aluminium
*Aluminium
*Chromium (ONLY RIE2!)
*Chromium (if needed)
*Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)
|-  valign="top"
!Etch rate
|
|
*Si<sub>3</sub>N<sub>4</sub> @ 180 <sup>o</sup>C: ~84 Å/min
*Photoresist
*Si<sub>3</sub>N<sub>4</sub> @ 160 <sup>o</sup>C: ~60 Å/min
*DUV resist
*E-beam resist
*Silicon Oxide
*Silicon Nitride
*Aluminium
*Chromium (if needed)
|
|
*PECVD nitride: ~400-1000 Å/min
*Photoresist
*DUV resist
*E-beam resist
*Silicon Oxide
*Silicon Nitride
*Aluminium
*Metals if they cover less than 5% of the wafer area
|
|
*Typically 40-50 nm/min can be increased or decreased by using other recipe parameters. 
*Any material that is accepted in the machine
|- valign="top"
!Batch size
|
|
*1-25 wafers at a time
*Resists
*other materials from the allowed list of materials
|-
 
|-
|-style="background:WhiteSmoke; color:black"
!Etch rate range
|
*Si<sub>3</sub>N<sub>4</sub> @ 160 <sup>o</sup>C: ~26 Å/min
|
*PECVD nitride: ~40.0-100.0 nm/min
*Stoichiometric LPCVD nitride: ~0.65-8 nm/min <!-- Copyrigth issues kabi (''Yannick Seis, KU, 2019'')-->
|
|
*1-25 wafers at a time
*Process dependent.
*From 0 to ~300 nm/min
|
|
*1 wafer at a time
*Process dependent.
|- valign="top"
*from 0 to ~500 nm/min
!Size of substrate
|
|
*4" wafers
*Probably between 20-300 nm/min depending on the process parameters
|
|
*4" wafers
*Process dependent.
*Has not been tested yet.
|
|
*4" wafers or smaller pieces
*Process dependent
|- valign="top"
*60-65 nm/min has been tested
!Allowed materials
|-
 
|-
|-style="background:LightGrey; color:black"
!Substrate size
|
*<nowiki>#</nowiki>1-25 4" and 6" wafers
|
*<nowiki>#</nowiki>1-25 4"-6" wafers  
|
*As many small samples as can be bonded on a 150mm wafer
*50 mm wafers if bonded on a 150mm wafer
*<nowiki>#</nowiki>1 100 mm wafer if bonded on a 150 mm wafer
*#1 150 mm wafer
|
*As many small samples as can be fitted on a 100mm wafer
*<nowiki>#</nowiki>1 50 mm wafer fitted on a 100mm wafer
*<nowiki>#</nowiki>1 100 mm wafer
|
*As many small samples as can be fitted on the 100mm carrier (bad/no cooling!)
*<nowiki>#</nowiki>1 100mm wafer (or smaller with carrier)
*<nowiki>#</nowiki>1 150mm wafer (only when the system is set up for 150mm)
|
*As many samples as can be securely fitted on a up to 200mm wafer
*<nowiki>#</nowiki>1 50 mm wafer with special carrier
*<nowiki>#</nowiki>1 100 mm wafer with special carrier
*<nowiki>#</nowiki>1 150 mm wafers with special carrier
*<nowiki>#</nowiki>1 200 mm wafer
|
*Set up for 150mm wafers
*Smaller samples can be processes when fixed to a 150mm carrier wafer.
|-
|-style="background:WhiteSmoke; color:black"
!'''Allowed materials'''
|
|
*Silicon
*Silicon
Line 80: Line 179:
*Silicon Oxynitride
*Silicon Oxynitride
*Photoresist
*Photoresist
*E-beam resist
*E-beam resists
*DUV resists
*Aluminium (only for masking
*Chromium (only for masking and on the back side if fused silica)
*Quartz/fused silica
|
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*E-beam resists
*DUV resists
*Aluminium
*Aluminium
*Chromium (ONLY RIE2!)
*Chromium (only for masking and on the back side if fused silica)
*Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)
*Quartz/fused silica
|
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*E-beam resists
*DUV resists
*Other metals if they cover less than 5% of the wafer area
*Quartz/fused silica
|
*Silicon
*Silicon oxides
*Silicon (oxy)nitrides
*Metals from the +list
*Metals from the -list
*Alloys from the above list
*Stainless steel
*Glass
*III-V materials
*Resists
*Polymers
*Capton tape
|
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*E-beam resists
*DUV resists
*Aluminium (Al, Al2O3, AlN)
*Chromium
*Titanium (Ti, TiW, TiN, TiO2)
*Tungsten (W)
*Molybdynem
*Quartz/fused silica
|-
|-
|}
|}
<br clear="all" />

Latest revision as of 09:46, 26 March 2025

Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.

All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.

Feedback to this page: click here

Comparing silicon nitride etch methods at DTU Nanolab

There are a broad variety of silicon nitride etch methods at DTU Nanolab. The methods are compared here to make it easier for you to compare and choose the one that suits your needs.


Compare the methods for Silicon Nitride etching

Wet Silicon Nitride Etch BHF Pegasus 4 AOE (Advanced Oxide Etch) ASE IBE/IBSD Ionfab 300 ICP Metal


Generel description
  • Isotropic etch
  • Well suited for removing all nitride on a wafer surface (nitride strip) without a mask. High selectivity Si3N4/Si (>100) and Si3N4/SiO2 (>20) @ 160 C.
  • Isotropic etch
  • Well suited for removing all PECVD nitride on a wafer surface (nitride strip) without a mask. Etches LPCVD nitride very slowly
  • Anisotropic etch: vertical sidewalls
  • With cassette loader for batch processing.
  • Anisotropic etch: vertical sidewalls
  • Deep etch
  • Anisotropic etch: vertical sidewalls
  • Primarily for samples with small amounts of metal
  • Primarily for pure physical etch by sputtering with Ar-ions
  • Anisotropic etch: vertical sidewalls
  • Primarily for Cl/Br etch chemistry.
  • F-chemistry, please use AOE or Pegasus 4.
Possible masking materials
  • Silicon Oxide
  • PolySilicon
  • Photoresist
  • PolySilicon
  • Blue film
  • Photoresist
  • DUV resist
  • E-beam resist
  • Silicon Oxide
  • Silicon Nitride
  • Aluminium
  • Chromium (if needed)
  • Photoresist
  • DUV resist
  • E-beam resist
  • Silicon Oxide
  • Silicon Nitride
  • Aluminium
  • Chromium (if needed)
  • Photoresist
  • DUV resist
  • E-beam resist
  • Silicon Oxide
  • Silicon Nitride
  • Aluminium
  • Metals if they cover less than 5% of the wafer area
  • Any material that is accepted in the machine
  • Resists
  • other materials from the allowed list of materials
Etch rate range
  • Si3N4 @ 160 oC: ~26 Å/min
  • PECVD nitride: ~40.0-100.0 nm/min
  • Stoichiometric LPCVD nitride: ~0.65-8 nm/min
  • Process dependent.
  • From 0 to ~300 nm/min
  • Process dependent.
  • from 0 to ~500 nm/min
  • Probably between 20-300 nm/min depending on the process parameters
  • Process dependent.
  • Has not been tested yet.
  • Process dependent
  • 60-65 nm/min has been tested
Substrate size
  • #1-25 4" and 6" wafers
  • #1-25 4"-6" wafers
  • As many small samples as can be bonded on a 150mm wafer
  • 50 mm wafers if bonded on a 150mm wafer
  • #1 100 mm wafer if bonded on a 150 mm wafer
    1. 1 150 mm wafer
  • As many small samples as can be fitted on a 100mm wafer
  • #1 50 mm wafer fitted on a 100mm wafer
  • #1 100 mm wafer
  • As many small samples as can be fitted on the 100mm carrier (bad/no cooling!)
  • #1 100mm wafer (or smaller with carrier)
  • #1 150mm wafer (only when the system is set up for 150mm)
  • As many samples as can be securely fitted on a up to 200mm wafer
  • #1 50 mm wafer with special carrier
  • #1 100 mm wafer with special carrier
  • #1 150 mm wafers with special carrier
  • #1 200 mm wafer
  • Set up for 150mm wafers
  • Smaller samples can be processes when fixed to a 150mm carrier wafer.
Allowed materials
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • Blue film
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resists
  • DUV resists
  • Aluminium (only for masking
  • Chromium (only for masking and on the back side if fused silica)
  • Quartz/fused silica
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resists
  • DUV resists
  • Aluminium
  • Chromium (only for masking and on the back side if fused silica)
  • Quartz/fused silica
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resists
  • DUV resists
  • Other metals if they cover less than 5% of the wafer area
  • Quartz/fused silica
  • Silicon
  • Silicon oxides
  • Silicon (oxy)nitrides
  • Metals from the +list
  • Metals from the -list
  • Alloys from the above list
  • Stainless steel
  • Glass
  • III-V materials
  • Resists
  • Polymers
  • Capton tape
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resists
  • DUV resists
  • Aluminium (Al, Al2O3, AlN)
  • Chromium
  • Titanium (Ti, TiW, TiN, TiO2)
  • Tungsten (W)
  • Molybdynem
  • Quartz/fused silica