Specific Process Knowledge/Thin film deposition/Deposition of Alumina: Difference between revisions
Appearance
No edit summary |
|||
| (25 intermediate revisions by 5 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Alumina click here]''' | ||
''All text by Nanolab staff'' | |||
==Deposition of | ==Deposition of Al<sub>2</sub>O<sub>3</sub>== | ||
Aluminium oxide (Alumina) can be deposited by use of ALD (atomic layer deposition) or by | Aluminium oxide (Alumina, Al<sub>2</sub>O<sub>3</sub>) can be deposited by use of ALD (atomic layer deposition), by e-beam evaporation or by sputtering. During the evaporation or sputter deposition oxygen is added to the chamber resulting in aluminium oxide on the sample. | ||
*[[Specific Process Knowledge/Thin film deposition/Lesker| | *[[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/Al2O3_deposition_using_ALD|Al<sub>2</sub>O<sub>3</sub> deposition using ALD]] | ||
*[[ | *[[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System(Lesker)]] | ||
*[[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|Sputter-System Metal-Oxide(PC1)]] | |||
*[[Specific_Process_Knowledge/Thin_film_deposition/Deposition of Alumina/E-beam Evaporation of Al2O3 in Temescal-2|Evaporation of Al<sub>2</sub>O<sub>3</sub> in E-Beam Evaporator (10-pockets)]] | |||
==Comparison of the methods for deposition of | ==Comparison of the methods for deposition of Alumium Oxide== | ||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | ||
|- | |- | ||
| Line 17: | Line 19: | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
! | ! | ||
![[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System(Lesker)]] | |||
![[Specific Process Knowledge/Thin film deposition/Lesker|Sputter System Lesker]] | ![[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system|Sputter-System Metal-Oxide(PC1)]] | ||
![[ | |||
![[Specific Process Knowledge/Thin film deposition/ALD Picosun R200|ALD Picosun 200]] | ![[Specific Process Knowledge/Thin film deposition/ALD Picosun R200|ALD Picosun 200]] | ||
![[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|10-pocket e-beam evaporator]] | |||
|- | |- | ||
| Line 27: | Line 29: | ||
!Generel description | !Generel description | ||
| | | | ||
* | *RF sputtering from Al<sub>2</sub>O<sub>3</sub> target | ||
*Reactive sputtering | |||
| | | | ||
* | *RF sputtering from Al<sub>2</sub>O<sub>3</sub> target | ||
* | *Pulsed DC reactive sputtering | ||
*Reactive HIPIMS (high-power impulse magnetron sputtering) | |||
| | | | ||
* | *ALD (atomic layer deposition) of Al<sub>2</sub>O<sub>3</sub> | ||
| | | | ||
* | *E-beam evaporation of Al<sub>2</sub>O<sub>3</sub> pellets or of Al in an O<sub>2</sub> flow | ||
|- | |- | ||
| Line 41: | Line 45: | ||
!Stoichiometry | !Stoichiometry | ||
| | | | ||
* | *Not tested | ||
| | | | ||
* | *Not tested | ||
| | | | ||
* | *Al<sub>2</sub>O<sub>3</sub>, very good | ||
| | | | ||
* | *Not tested yet | ||
|- | |- | ||
| Line 54: | Line 58: | ||
!Film Thickness | !Film Thickness | ||
| | | | ||
* | *few nm - 200 nm | ||
| | | | ||
* | *few nm - 200-300 nm | ||
| | | | ||
* | * 0nm - 100 nm | ||
| | | | ||
* | *few nm - 200 nm (talk to staff if you wish to deposit more than 100 nm as it can cause flaking in the chamber) | ||
|- | |- | ||
| Line 66: | Line 70: | ||
!Deposition rate | !Deposition rate | ||
| | | | ||
* | * 0.3 nm/min | ||
| | | | ||
* | * About 1.7 nm/min, depends on sputtering parameters | ||
| | | | ||
* | *0.088 - 0.097 nm/cycle (Using the "Al2O3" recipe, temperature dependent) | ||
| | | | ||
* | * 1-2 Å/s | ||
|- | |- | ||
| Line 80: | Line 83: | ||
!Step coverage | !Step coverage | ||
| | | | ||
* | *unknown | ||
| | | | ||
* | *unknown | ||
| | | | ||
* | *Very good. Covers sample everywhere (but long purge time needed for very high aspect ratio structures) | ||
| | | | ||
* | * We expect no step coverage unless using tilt holder, in which case the step coverage can be very good and can be tuned. | ||
|- | |- | ||
| Line 92: | Line 95: | ||
!Process Temperature | !Process Temperature | ||
| | | | ||
* | * room temperature | ||
| | | | ||
* | * Up to 600 °C | ||
| | | | ||
* | *150 °C - 350 °C | ||
| | | | ||
* | * Up to 250 °C | ||
|- | |- | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!More info on | !More info on Al<sub>2</sub>O<sub>3</sub> | ||
| | | | ||
| | | | ||
* | *See [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|deposition conditions]] | ||
| | | | ||
* | *[[Specific Process Knowledge/Thin film deposition/ALD Picosun R200/Al2O3 deposition using ALD|Al<sub>2</sub>O<sub>3</sub> deposition using ALD]] | ||
| | | | ||
|- | |- | ||
| Line 120: | Line 120: | ||
!Substrate size | !Substrate size | ||
| | | | ||
* | * chips | ||
* 1x 100 mm wafer | |||
* | * 1x 150 mm wafer | ||
* | |||
| | | | ||
* | * chips | ||
* | * 10x 100 mm wafer | ||
* 10x 150 mm wafer | |||
* | |||
| | | | ||
*1-5 100 mm wafers | *1-5 100 mm wafers | ||
*1-5 150 mm wafers | *1-5 150 mm wafers | ||
*1-3 200 mm wafers | |||
*Several smaller samples | *Several smaller samples | ||
| | |||
* chips | |||
* 1-3 x 100 mm wafers | |||
* 1-3 x 150 mm wafers | |||
* 1-3 x 200 mm wafers | |||
|- | |- | ||
| Line 143: | Line 143: | ||
!'''Allowed materials''' | !'''Allowed materials''' | ||
| | | | ||
* | *almost any that does not degas | ||
| | | | ||
* | *almost any that does not degas. Note special carrier for III-V materials. See [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 cross-contamination sheet]. | ||
| | | | ||
*Silicon | *Silicon | ||
| Line 158: | Line 155: | ||
*III-V materials (use dedicated carrier wafer) | *III-V materials (use dedicated carrier wafer) | ||
*Polymers (depending on the melting point/deposition temperature, use carrier wafer) | *Polymers (depending on the melting point/deposition temperature, use carrier wafer) | ||
| | |||
*almost any that does not degas. See [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=511 cross-contamination sheet] | |||
|- | |- | ||
|} | |} | ||