Jump to content

LabAdviser/314/Microscopy 314-307/SEM/QFEG: Difference between revisions

From LabAdviser
Afull (talk | contribs)
Mktracy (talk | contribs)
 
(71 intermediate revisions by 3 users not shown)
Line 1: Line 1:
= QFEG 200 Cryo ESEM (FEI)=
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=LabAdviser/314/Microscopy_314-307/SEM/QFEG click here]'''


[[Image:FEG.jpg|300x300px|right|thumb| DTU Nanolabs QFEG positioned in building 314 room no. 010]]
''This section is written by DTU Nanolab internal if nothing else is stated.''
[[Category:314]]
[[Category:314-Microscopy]]
__FORCETOC__
=QFEG 200 Cryo ESEM (FEI Quanta FEG 200)=


[[File:202231020_IMG_4763.jpg|400px|right|thumb| DTU Nanolab QFEG located in building 307 room 907]]


The QFEG 200 Cryo is an FEI Quanta FEG (Field Emission Gun) scanning electron microscope with a spatial resolution of 2 nm for the ETD detector in high vacuum at 30 keV. The microscope can operate in several modes, such as high vacuum, low vacuum, environmental mode, room temperature, low temperature and cryo. Our QFEG is fitted with an EDS detector, which allows for analytical measurements in all the operation modes. With the cryo transfer system available, it is especially suited for cryo experiments.
The QFEG 200 Cryo is an FEI Quanta FEG (Field Emission Gun) scanning electron microscope with a spatial resolution of 2 nm for the ETD detector in high vacuum at 30 keV. The microscope can operate in several modes, such as high vacuum, low vacuum, environmental mode, room temperature, low temperature and cryo. Our QFEG is fitted with an EDS detector, which allows for analytical measurements in all the operation modes. With the cryo transfer system available, it is especially suited for cryo experiments.


== Process information ==
= Process information =


*'''Electron source'''
*'''Electron source'''
Line 23: Line 28:
Quorum PP2000 Cryo System, FEI Peltier stage (-10°C to 22°C).
Quorum PP2000 Cryo System, FEI Peltier stage (-10°C to 22°C).


==Equipment performance and process related parameters==
=Equipment performance and process related parameters=
{| border="2" cellspacing="0" cellpadding="0"  
{| border="2" cellspacing="0" cellpadding="0"  
!colspan="2" border="none" style="background:silver; color:black;" align="center |Equipment  
!colspan="2" border="none" style="background:silver; color:black;" align="center |Equipment  
|style="background:WhiteSmoke; color:black" align="center"|FEI QFEG 200 Cryo ESEM
|style="background:WhiteSmoke; color:black" align="center"|QFEG Cryo SEM FEI Quanta FEG 200
|-
|-
!style="background:silver; color:black;" align="center" width="60"| Purpose  
!style="background:silver; color:black;" align="center" width="60"| Purpose  
Line 33: Line 38:
* Vizualization of surfaces (topography and Z contrast)  
* Vizualization of surfaces (topography and Z contrast)  
* Vizualization of projected image (BF STEM image)
* Vizualization of projected image (BF STEM image)
* Energy Dispersive X-ray analysis
* Energy Dispersive X-ray analysis (EDS)
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Performance
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Performance
Line 81: Line 86:
* High vacuum (10<sup>-4</sup> Pa), Low vacuum and Enviromental mode (up to 2700Pa)
* High vacuum (10<sup>-4</sup> Pa), Low vacuum and Enviromental mode (up to 2700Pa)
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Samples
|style="background:LightGrey; color:black"|Sample sizes
|style="background:LightGrey; color:black"|Sample sizes
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* No actual limit (limitted by stage movment and detector position).
* No actual limit (limitted by stage movement and detector position).
|-
|-
| style="background:LightGrey; color:black"|Allowed materials
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* Conductors, Semiconductors,Insulators,Wet Samples, Biological (not pathogents!)
* Conductors, Semiconductors,Insulators,Wet Samples, Biological (not pathogens!)
|-  
|-  
|}
|}




'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=LabAdviser/314/SEM/QFEG click here]'''
= Examples of the QFEG's capabilities =
 
''All images are taken by Marie Karen Tracy Hong Lin @DTU Nanolab''
 
== SEM (Scanning Electron Microscopy) ==
The SEM is a remarkable technique which can offer information such as the surface morphology of a sample and also a 3D appearance of the specimen. It can offer the best resolution (2 nm at 30kV) at high magnification and also topographical details because of its great depth of field.
 
[[File:20201017_Microalgae_Image01_018-1.jpg|500px|left|thumb|SEM imaging of Microalgae with gold nanoparticles]]<br clear="all" />
[[File:20191217 Bacteria Image_032-1.jpg|500px|left|thumb|SEM imaging of Bacteria]]<br clear="all" />
[[File:Spider_006-1.jpg|500px|left|thumb|SEM imaging of Spider]]<br clear="all" />
[[File:Spider Web_020-1.jpg|500px|left|thumb|SEM imaging of Spider web]]<br clear="all" />
 
== BSD (Backscattered Electron Detector) ==
[[File:20201017_Microalgae_Image01_019-1.jpg|500px|left|thumb|BSD imaging of Microalgae with gold nanoparticles]]<br clear="all" />
 
 
== STEM (Scanning Transmission Electron Microscopy) ==
STEM combines the principles of transmission electron microscopy and scanning electron microscopy and can be performed on either type of instrument. In the STEM setting, the sample requires to have a thickness of less than 200 nm for visualization. Sample preparation prior to STEM microscopy involve samples being embedded in epoxy resin and then ultra sectioning using the [[LabAdviser/314/Preparation_314-307/Soft-matter#Leica_EM_UC7_Ultramicrotome|Ultramicrotome]]. For more sensitive samples that need to be sectionned at cryogenic temperatures (below −180 °C), the [[LabAdviser/314/Preparation_314-307/Soft-matter#Leica_EM_FC7_Cryo-Ultramicrotome|Cryo-Ultramicrotome]] can be used for that purpose.
 
[[File:20210519_Microalgae_K2_007-1.jpg|500px|left|thumb|STEM imaging of a cross section of Microalgae, 100 nm thick section]]<br clear="all" />
[[File:20210413_Yeast_S1_005-1.jpg|500px|left|thumb|STEM imaging of a cross section of Yeast, 100 nm thick section]]<br clear="all" />
 
== ESEM (Environmental Scanning Electron Microscopy) ==
In the ESEM setting, sample temperature and specimen chamber vapour pressure can both be controlled thus allowing visualiztion of the specimen when heated, cooled, wetted or dried.
 
== Cryo-SEM ==
In the cryo-SEM setting, the sample is visualized in a frozen state (down to -190 °C). This setting is very useful when the specimen being observed needs visualiztion in its hydrated form. It can be imaged by using either the secondary electrons (SE) or backscattered electrons (BSE) detector.
 
[[File:Blue cheese_002-1.jpg|500px|left|thumb|Cryo-SEM imaging of Blue cheese]]<br clear="all" />
[[File:Cryo-SEM of Mucus in rat intestine-1.jpg|500px|left|thumb|Cryo-SEM imaging of Mucus in rat intestine]]<br clear="all" />
[[File:20220310_Lotus leaf_023-1.jpg|500px|left|thumb|Cryo-SEM imaging of plant leaf surface]]<br clear="all" />
 
== EDS (Energy Dispersive X-ray Spectroscopy) ==
The EDS is an analytical technique which can provide elemental or chemical characteristics of a sample.
 
[[File:EDS Bacteria and Au nanoparticle.JPG|1000px|left|thumb|EDS mapping of bacteria and gold nanoparticle]]<br clear="all" />
 
[[File:Microalgae with iron nanoparticles .jpg|1000px|left|thumb|SEM analysis and EDS mapping of microalgae with iron nanoparticles]]<br clear="all" />

Latest revision as of 10:59, 5 December 2024

Feedback to this page: click here

This section is written by DTU Nanolab internal if nothing else is stated.

QFEG 200 Cryo ESEM (FEI Quanta FEG 200)

DTU Nanolab QFEG located in building 307 room 907

The QFEG 200 Cryo is an FEI Quanta FEG (Field Emission Gun) scanning electron microscope with a spatial resolution of 2 nm for the ETD detector in high vacuum at 30 keV. The microscope can operate in several modes, such as high vacuum, low vacuum, environmental mode, room temperature, low temperature and cryo. Our QFEG is fitted with an EDS detector, which allows for analytical measurements in all the operation modes. With the cryo transfer system available, it is especially suited for cryo experiments.

Process information

  • Electron source

Field emission gun

  • Accelerating voltage

500 V- 30 kV

  • Resolution

2 nm at 30 kV (SE)

  • Imaging detectors

Everhart-Thornley (SE/BSE), Solid State BSE, Large Field, Gaseous SE, Gaseous BSE, Gaseous Analytical, STEM, vCD and CCD Camera

  • Imaging modes

High, low vacuum and environmental

  • Analytical capabilities

Energy dispersive X-rays (Oxford Instruments 80 mm2 X-Max silicon drift detector, MnKα resolution at 124 eV)

  • Attachments

Quorum PP2000 Cryo System, FEI Peltier stage (-10°C to 22°C).

Equipment performance and process related parameters

Equipment QFEG Cryo SEM FEI Quanta FEG 200
Purpose Vizualization and Microanalysis
  • Vizualization of surfaces (topography and Z contrast)
  • Vizualization of projected image (BF STEM image)
  • Energy Dispersive X-ray analysis (EDS)
Performance Resolution The resolution of QFEG dependends on the sample and the operation mode!
  • 2 nm at 30 keV for Au on C sample with the ETD detector
Instrument specifics Detectors
  • ETD- Everhart-Thornley for secondary electrons
  • BSD- Solid state Back Scattered Detector
  • LFD- Large Field Detector for secondary electrons
  • GSED- Gaseous Secondary Electron Detector
  • GBSD- Gaseous Backscattered Electron Detector
  • GAD- Gaseous Analystical Detector
  • STEM- right field Scanning Tramission Electron detector
  • vCD- low voltage BSED
  • CCD camera
Electron source
  • Field Emission - Tungsten filament
Stage (room temperature)
  • X, Y: 25 × 25 mm
  • T: 0 to 60o (Full tilt require removment of cryo cold trap.)
  • R: 360o
Peltier stage
  • FEI Peltier stage -10o to 22o
Cryo stage
  • Quorum PP2000 Cryo System
EDS
  • Oxford Instruments 80 mm2 X-Max silicon drift detector, MnKα resolution at 124 eV
Operating pressures
  • High vacuum (10-4 Pa), Low vacuum and Enviromental mode (up to 2700Pa)
Samples Sample sizes
  • No actual limit (limitted by stage movement and detector position).
Allowed materials
  • Conductors, Semiconductors,Insulators,Wet Samples, Biological (not pathogens!)


Examples of the QFEG's capabilities

All images are taken by Marie Karen Tracy Hong Lin @DTU Nanolab

SEM (Scanning Electron Microscopy)

The SEM is a remarkable technique which can offer information such as the surface morphology of a sample and also a 3D appearance of the specimen. It can offer the best resolution (2 nm at 30kV) at high magnification and also topographical details because of its great depth of field.

SEM imaging of Microalgae with gold nanoparticles


SEM imaging of Bacteria


SEM imaging of Spider


SEM imaging of Spider web


BSD (Backscattered Electron Detector)

BSD imaging of Microalgae with gold nanoparticles



STEM (Scanning Transmission Electron Microscopy)

STEM combines the principles of transmission electron microscopy and scanning electron microscopy and can be performed on either type of instrument. In the STEM setting, the sample requires to have a thickness of less than 200 nm for visualization. Sample preparation prior to STEM microscopy involve samples being embedded in epoxy resin and then ultra sectioning using the Ultramicrotome. For more sensitive samples that need to be sectionned at cryogenic temperatures (below −180 °C), the Cryo-Ultramicrotome can be used for that purpose.

STEM imaging of a cross section of Microalgae, 100 nm thick section


STEM imaging of a cross section of Yeast, 100 nm thick section


ESEM (Environmental Scanning Electron Microscopy)

In the ESEM setting, sample temperature and specimen chamber vapour pressure can both be controlled thus allowing visualiztion of the specimen when heated, cooled, wetted or dried.


Cryo-SEM

In the cryo-SEM setting, the sample is visualized in a frozen state (down to -190 °C). This setting is very useful when the specimen being observed needs visualiztion in its hydrated form. It can be imaged by using either the secondary electrons (SE) or backscattered electrons (BSE) detector.

Cryo-SEM imaging of Blue cheese


Cryo-SEM imaging of Mucus in rat intestine


Cryo-SEM imaging of plant leaf surface


EDS (Energy Dispersive X-ray Spectroscopy)

The EDS is an analytical technique which can provide elemental or chemical characteristics of a sample.

EDS mapping of bacteria and gold nanoparticle


SEM analysis and EDS mapping of microalgae with iron nanoparticles