Specific Process Knowledge/Lithography/Development: Difference between revisions

From LabAdviser
Taran (talk | contribs)
Jehem (talk | contribs)
 
(218 intermediate revisions by 7 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development click here]'''
{{cc-nanolab}}


=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Development click here]'''


[[Category: Equipment|Lithography development]]
[[Category: Lithography|Development]]


==Coaters: Comparison Table==
__TOC__


{| border="2" cellspacing="0" cellpadding="2"  
==Development Comparison Table==
 
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  


!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer-1 and Developer-2|Developer 1 and 2]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer: SU8 (Wet Bench)|Developer: SU8 (Wet bench)]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer-6inch|Developer-6inch]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer: E-beam 02|Developer: E-beam 02]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#SU8-Developer|SU8-Developer]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer:_TMAH_Manual 02|Developer: TMAH Manual 02]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer-TMAH|Developer-TMAH]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|Developer: TMAH UV-lithography]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development/DUV_developer#Developer:_TMAH_Stepper|Developer: TMAH Stepper]]</b>


|-
|-
!style="background:silver; width:100px; color:black;" align="center"|Purpose  
!style="background:silver; color:black" align="center" width="60"|Purpose  
|style="background:LightGrey; color:black"|  
|style="background:LightGrey; color:black"|
 
 
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Coating and baking of
Development of:
**AZ5214E resist
*SU-8
**AZ4562 resist
**E-beam resist
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Coating and baking of
Development of:
**AZ5214E resist
*ZEP 520A
**AZ4562 resist
*AR-P 6200.xx (CSAR)
**SU8 resist
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Coating and baking of
Development of:
**SU8 resist
*AZ nLOF
*AZ MiR 701
*AZ 5214E
*AZ 4562
*DUV resists
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*In-line substrate HMDS priming
Development of:
*Coating and baking of
*AZ nLOF
**AZ MiR 701 (29cps) resist
*AZ MiR 701
**AZ nLOF 2020 resist
*AZ 5214E
*Post-exposure baking at 110°C
*AZ 4562
*DUV resists
Post-exposure baking
|style="background:WhiteSmoke; color:black"|
Development of:
*DUV resists
Post-exposure baking


|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Performance
!style="background:silver; color:black" align="center" width="60"|Developer
|style="background:LightGrey; color:black"|Substrate handling
|style="background:LightGrey; color:black"|
 
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* Cassette-to-cassette
mr-Dev 600 (PGMEA)
* Edge handling chuck
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* Single substrate
*ZED N-50
* Non-vacuum chuck for fragile substrates
*AR-600-546
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* Cassette-to-cassette
AZ 726 MIF (2.38% TMAH in water)
|style="background:WhiteSmoke; color:black"|
AZ 726 MIF (2.38% TMAH in water)
|style="background:WhiteSmoke; color:black"|
AZ 726 MIF (2.38% TMAH in water)
 
|-
|-
|style="background:LightGrey; color:black"|Permanent media
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black"|
Submersion
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* AZ5214E resist
Spray/Puddle
* AZ4562 resist
* Acetone for chuck cleaning
* Acetone for drip pan
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* AZ5214E resist
Puddle
* PGMEA for edge bead removal
* Acetone for chuck cleaning
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* AZ MiR 701 (29cps) resist
Puddle
* AZ nLOF 2020 resist
|style="background:WhiteSmoke; color:black"|
* PGMEA for backside rinse and edge-bead removal
Puddle
* PGMEA for spinner bowl cleaning and vapor tip bath
|-
|-
|style="background:LightGrey; color:black"|Manual dispense option
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* 2 automatic syringes
*Single wafer carrier
*Chip bucket
*100 mm carrier for up to 6 wafers
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* yes
*Vacuum chuck for 100 mm & 150 mm substrates
* pneumatic dispense for SU8 resist
*Chip chuck for chips & 2" substrates
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* no
*Vacuum chuck for 100 mm & 150 mm substrates
*Chip chuck for chips & 2" substrates
|style="background:WhiteSmoke; color:black"|
Vacuum chuck
|style="background:WhiteSmoke; color:black"|
Vacuum chuck
|-


!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameter range
|style="background:LightGrey; color:black"|Agitation
|style="background:LightGrey; color:black"|Spindle speed
 
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*100-5000 rpm
Magnetic stirrer
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*100-5000 rpm
Rotation
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*10 - 9990 rpm
Rotation
|style="background:WhiteSmoke; color:black"|
Rotation
|style="background:WhiteSmoke; color:black"|
Rotation
|-
|-
|style="background:LightGrey; color:black"|Gyrset
|style="background:LightGrey; color:black"|Rinse
 
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*optinal
IPA
|style="background:WhiteSmoke; color:black"|
IPA
|style="background:WhiteSmoke; color:black"|
DI water
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*optinal
DI water
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*no
DI water


|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:LightGrey; color:black"|Substrate size
 
|style="background:WhiteSmoke; color:black"|
* Chips
* 50 mm wafers
* 100 mm wafers
* 150 mm wafers
* 200 mm wafers
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*50 mm wafers
* Chips (5mm to 2")
*100 mm wafers
* 50 mm wafers
*150 mm wafers
* 100 mm wafers
* 150 mm wafers
|style="background:WhiteSmoke; color:black"|
* Chips (5mm to 2")
* 100 mm wafers
* 150 mm wafers
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*100 mm wafer
* 100 mm wafers
*150 mm wafer
* 150 mm wafers
* 200 mm wafers (may require tool change)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*100 mm wafers
* 100 mm wafers
*150 mm wafers (tool change required)
* 150 mm wafers
* 200 mm wafers (may require tool change)
|-
|-
|style="background:LightGrey; color:black"|Batch size
|style="background:LightGrey; color:black"|Allowed materials
 
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*1-24
*Silicon and glass substrates
*Film or pattern of all but Type IV
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*1
All cleanroom approved materials
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*1-25
*All cleanroom approved materials
|-
*Film or pattern of all types
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*All cleanroom materials except III-V materials
*Silicon and glass substrates
*Film or pattern of all but Type IV
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*All cleanroom materials except III-V materials
*Silicon, III-V, and glass substrates
|style="background:WhiteSmoke; color:black"|
*Film or pattern of all but Type IV
*Silicon
|-
*Glass
|style="background:LightGrey; color:black"|Batch
 
|style="background:WhiteSmoke; color:black" align="center"|
1 - 6
|style="background:WhiteSmoke; color:black" align="center"|
1
|style="background:WhiteSmoke; color:black" align="center"|
1
|style="background:WhiteSmoke; color:black" align="center"|
1 - 25
|style="background:WhiteSmoke; color:black" align="center"|
1 - 25
|-  
|-  
|}
|}
<br clear="all" />
<br clear="all" />


<!-- TARAN 2020-03-05
==Developer-1 and Developer-2==
==Developer-1 and Developer-2==
[[Image:Developer1&2.jpg|300 × 300px|thumb|right|Developer-1 (right) and Developer-2 (left) are located in C-1]]
[[Image:Developer1&2.jpg|300x300px|thumb|right|Developer-1 (right) and Developer-2 (left) are located in C-1]]


'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer-1_and_Developer-2 click here]'''
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer-1_and_Developer-2 click here]'''


Developer-1 and Developer-2
===<span style="color:red">This equipment was decommissioned January 2017!</span>===


'''The user APV, and contact information can be found in LabManager: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=62 Developer-1] [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=63 Developer-2]'''
Developer-1 and Developer-2 are manual developer baths for submersion development of AZ 5214E and AZ 4562 resists in AZ 351B developer. The developer is mixed 1:5 in water by the user prior to development start, and the wafer cassette is agitated manually by the user during development. The development time is controlled manually by the user. After development, the substrates are rinsed with water in the bench.
 
'''The user APV, and contact information can be found in LabManager: [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=62 Developer-1] [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=63 Developer-2]'''


===Process information===
===Process information===
*Before using one of developer baths, please check the "Litho4_Dev-7up-KOH" logbook to find out when they were last used. A fresh bath can be reused without problems.
*The main rule is a developer made yesterday must be changed.
*Rinse substrates with water for 4-5 min. after development.
*Spin-dry substrates or dry with nitrogen gun after rinsing.


'''Standard development time using vigorous agitation:'''
'''Standard development time using vigorous agitation:'''
Line 151: Line 221:
'''AZ 4562:'''
'''AZ 4562:'''
*10µm resist: 5 min
*10µm resist: 5 min
'''Standard development procedure:'''
*Before using one of developer baths, please check the "Litho4_Dev-7up-KOH" logbook to find out when they were last used. A fresh bath can be reused without problems.
*The main rule is a developer made yesterday must be changed.
*During development, agitate the substrates by moving the carrier up and down.
*Rinse substrates with water for 4-5 min. after development.
*Spin-dry substrates or dry with nitrogen gun after rinsing.


====Procedure for making a new developer====  
====Procedure for making a new developer====  


1. 800ml "Developer AZ 351B" is mixed with 4000ml water in a special container in the fume hood.  
1. Switch off the heater, and dump the old developer.


2. Fill the bath with the developer mixture and heat it to 22 °C before use.
2. 800ml "Developer AZ 351B" is mixed with 4000ml water in a special container in the fume hood.
 
3. Fill the bath with the developer mixture, and heat it to 22°C before use.


=== Equipment performance and process related parameters ===
=== Equipment performance and process related parameters ===
Line 164: Line 244:
!style="background:silver; color:black;" align="center" width="60"|Purpose  
!style="background:silver; color:black;" align="center" width="60"|Purpose  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
Development of
Development of
*AZ 5214E
*AZ 5214E
Line 176: Line 256:
(NaOH and sodium borate salt)
(NaOH and sodium borate salt)
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="1"|Method
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black" align="center"|
Submersion
Submersion
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameters
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black" align="center"|
Cassette
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black" align="center"|
Line 189: Line 273:
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black" align="center"|
Manual
Manual
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black" align="center"|
DI water
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
Line 208: Line 296:


<br clear="all" />
<br clear="all" />
-->


<!-- TARAN 2020-03-05
==Developer-6inch==
==Developer-6inch==


[[image:6inchDeveloper.jpg|300x300px|right|thumb|The Developer-6inch bench is located in E-5]]
[[image:6inchDeveloper.jpg|300x300px|right|thumb|The Developer: 6inch bench is located in E-4]]


'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Developers#Developer-6inch click here]'''
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Developers#Developer-6inch click here]'''


Spin Track 1 + 2 is an SVG 88 series track system from Rite Track. Each track consists of a HMDS priming module, a spin coating module, and a baking module. In fact, the only difference between the two tracks is the resist used in the spin coating module. Spin Track 1 + 2 is capable of handling 150 mm wafers, as well as 100 mm wafers, but is currently set up for 100 mm wafer processing.
===<span style="color:red">This equipment will be decommissioned December 2019!</span>===


The Spin Track 1 + 2 is controlled using the Recipe Manager software via the touchscreen on the arm attached to the lefthand end of the track. Recipes for the individual modules are developed by Danchip and combined into flows. The user selects a flow (specific to track 1 or 2), and the appropriate recipes will be downloaded and executed on the appropriate track. The other track runs an empty process (no wafers needed), and can unfortunately not be used by a second user while the first user is processing.
The Developer: 6inch bench is an automated developer bath for submersion development of AZ 5214E and AZ 4562 resists in AZ 351B developer. The developer is mixed 1:5 in water by the equipment prior to development start. The developer is circulated during development, and the wafer cassette may be agitated by a mechanical elevator. The development time is controlled manually by the user. After development, the substrates are rinsed with water in the bench.


'''The user manual, user APV, and contact information can be found in [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=189 LabManager]'''
'''The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=189 LabManager]'''


===Process information===
===Process information===
Line 227: Line 317:
'''AZ 5214E:'''
'''AZ 5214E:'''
*1.5µm resist: 60 sec
*1.5µm resist: 60 sec
*2.2µm resist: 70 sec
*4.2µm resist: 3 min
'''AZ 4562:'''
*10µm resist: 5 min


=== Equipment performance and process related parameters ===
=== Equipment performance and process related parameters ===
Line 234: Line 328:
!style="background:silver; color:black;" align="center" width="60"|Purpose  
!style="background:silver; color:black;" align="center" width="60"|Purpose  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
Development of
Development of
*AZ 5214E
*AZ 5214E
Line 246: Line 340:
(NaOH and sodium borate salt)
(NaOH and sodium borate salt)
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="1"|Method
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black" align="center"|
Submersion
Submersion
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameters
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black" align="center"|
Cassette
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black" align="center"|
Line 259: Line 357:
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black" align="center"|
Circulation and mechanical
Circulation and mechanical
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black" align="center"|
DI water
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
Line 279: Line 381:


<br clear="all" />
<br clear="all" />
-->


==SU8-Developer==
==Developer: SU8 (Wet Bench)==
[[Image:SU-8developer.jpg|300×300px|right|thumb|The SU8-Developer bench is located in C-1]]


'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#SU8-Developer click here]'''


The SU8-Developer bench is a manually operated chemical bench for submersion development of SU-8 photoresist in PGMEA (supplied in the cleanroom as mr-Dev 600). After development, the substrates are rinsed with IPA and dried in the bench.


'''The user manual, user APV, and contact information can be found in [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=154 LabManager]'''
[[Image:SU8dev.JPG|300x300px|right|thumb|The Developer: SU8(Wet Bench)is located in E-4 room.]]
 
The SU8-Developer bench is a manually operated wet bench for submersion development of SU-8 photoresist in PGMEA (supplied in the cleanroom as mr-Dev 600). The development process is in two stages; one bath (FIRST) to dissolve the bulk of the resist, and a second, cleaner bath (FINAL) to finish the development. The development time is controlled manually by the user. After development, the substrates are rinsed with IPA in dedicated IPA bath and put for drying in the empty bath.
 
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=509 LabManager: Developer: SU8(Wet Bench)] - '''requires login'''
 
===Process information===
Several aspects of the outcome of SU-8 processing are affected by the development process. The lithographic resolution is affected by the time between PEB (post-exposure bake) and development, as the cross-linking process continues in the interface between exposed and unexposed regions even at room temperature. Cracks in the structures is affected by two things; the development time, and how much has previously been developed in the developer bath. Cracking is worse with longer development time, and worst in a new developer bath. The effect of the developer use quickly saturates (5-10 wafers). Finally, the stability of fine structures (high aspect ratio) is affected by the rinse after development, as the lower surface tension of IPA compared to PGMEA reduces pattern collapse during drying.
 
 
Development time is strongly dependent on the SU-8 thickness.
*Minimum development time: 1 min per 20 µm in FIRST
 
 
Suggestions:
*2-5µm: 2 min. in FIRST; 2 min. in FINAL
*40µm: 5 min. in FIRST; 5 min. in FINAL (however, 3 min. in FIRST and 2 min. in FINAL is sufficient)
*180-250µm: 15 min. in FIRST; 15 min. in FINAL


=== Equipment performance and process related parameters ===
=== Equipment performance and process related parameters ===


{| border="2" cellspacing="0" cellpadding="2"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
 


!style="background:silver; color:black;" align="center" width="60"|Purpose  
!style="background:silver; color:black;" align="center" width="60"|Purpose  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
Development of
Development of:
*SU-8
*SU-8
|-
|-
!style="background:silver; color:black;" align="center" width="60"|Developer  
!style="background:silver; color:black;" align="center" width="60"|Developer  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
mr-Dev 600
mr-Dev 600


(PGMEA)
(PGMEA)
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="1"|Method
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Submersion
Submersion
|-
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black"|
Single wafer holder
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Room temperature
Room temperature
|-
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Magnetic stirrer
Magnetic stirrer
|-
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
IPA
IPA
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
* 100 mm wafers
*100 mm wafers
*150 mm wafers, check the liquid level in the baths
*200 mm wafer, check the liquid level in the baths
|-
|-
| style="background:LightGrey; color:black"|Allowed materials
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Silicon and glass substrates
*Silicon and glass substrates
*Film, or pattern, of all materials except Type IV
|-
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black"|
1-6
|-
|}
 
<br clear="all" />
 
==Developer: E-beam 02==
[[Image:IMG 2464.JPG|300×300px|right|thumb|Developer: E-beam 02 is located in E-4]]
 
Developer: E-beam 02 is a manually operated, single substrate puddle developer. It uses the ZED-N50 or AR 600-50 developers and IPA for rinsing. The substrates are loaded manually one by one into the developer. Developer dispense, puddle time, IPA rinse, and drying is then performed automatically by the equipment.
 
'''[https://www.youtube.com/watch?v=btinNzYnLnY Training video]''' (for Developer: TMAH Manual, but it is the same model)
 
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=324 LabManager] - '''requires login'''
 
===Process information===
All recipes use the following structure:
#Pressurize the developer canister
#Dispense puddle while rotating substrate slowly
#Puddle development while not rotating
#Agitate substrate once per 15 seconds by rotating slowly for 1 second
#Spin off developer
#Clean substrate with IPA
#Dry substrate and chamber with nitrogen
 
Multi-puddle recipes repeat steps 2-5 for the given number of puddles.
 
 
'''Process recipes'''<br>
N50 recipes have the letter "N" in them. AR-600-50 recipes have the letter "A"  in them. The number is the development time in seconds:
*01 Rinse
*02 N 15
*03 N 30
*04 N 60
*05 N 90
*06 N 120
*07 N 180
*08 N 300
*09 N 600
*10 N 2x60
*11 N 5x60
*12 A 15
*13 A 30
*14 A 60
*15 A 90
*16 A 120
*17 A 180
*18 A 300
*19 A 600
*20 A 2x60
*21 A 5x60
 
=== Equipment performance and process related parameters ===
 
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
 
|-
!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
Development of:
*CSAR
*ZEP520A


Film or pattern of all but Type IV
|-
|-
|style="background:LightGrey; color:black"|Batch
!style="background:silver; color:black;" width="60"|Developer
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:LightGrey; color:black"|
1-8
|style="background:WhiteSmoke; color:black"|
*AR 600-50
*ZED N-50
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black"|
Puddle
|-
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black"|
*Chip chuck for chips
*Non-vacuum chuck for 2" wafers
*Non-vacuum chuck for 100 mm and 150 mm wafers
*Non-vacuum chuck for 200 mm wafers
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black"|
1 second rotational agitation at 30 rpm every 15 seconds
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black"|
IPA
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black"|
*Chips
*2" wafers
*100 mm wafers
*150 mm wafers
*200 mm wafers
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
*All cleanroom approved materials
*Film, or pattern, of all materials except Type IV
|-
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
1
|-  
|-  
|}
|}
Line 344: Line 577:
<br clear="all" />
<br clear="all" />


==Developer-TMAH==
==Developer: TMAH Manual 02==
[[Image:KSspinner.JPG|300×300px|right|thumb|Developer-TMAH is located in C-1]]
[[Image:IMG 2464.JPG|300×300px|right|thumb|Developer: TMAH Manual 02 is located in E-4]]
 
Developer: TMAH Manual 02 is a manually operated, single substrate or chip puddle developer. It uses the TMAH based AZ 726 MIF developer (2.38 % TMAH in  water with a small amount of wetting agent). The substrates or chips are loaded manually one by one into the developer. Developer dispense, puddle time, water rinse, and drying is performed automatically by the equipment.
 


'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer-TMAH click here]'''
'''[https://www.youtube.com/watch?v=btinNzYnLnY Training video]'''


Developer-TMAH is a manually operated, single substrate spray-puddle developer. It uses the TMAH based AZ 726 MIF developer (2.38 % TMAH in  water with a small amount of wetting agent).


'''The user manual, user APV, and contact information can be found in [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=324 LabManager]'''
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=324 LabManager] - '''requires login'''
 
===Process information===
All recipes use the following structure:
#Pressurize the TMAH canister
#Dispense puddle while rotating substrate slowly
#Puddle development while not rotating
#Agitate substrate once per 15 seconds by rotating slowly for 1 second
#Spin off developer
#Clean substrate and chamber with DI water
#Dry substrate and chamber with nitrogen
 
Multi-puddle recipes repeat steps 2-5 for the given number of puddles.
 
 
'''Process recipes'''<br>
SP: Single-puddle<br>
MP: Multi-puddle
 
*01 Rinse
*02 SP 15
*03 SP 30
*04 SP 60
*05 SP 90
*06 SP 120
*07 SP 300
*08 MP 2x60
*09 MP 5x60
*91 SP test
*92 MP test


=== Equipment performance and process related parameters ===
=== Equipment performance and process related parameters ===


{| border="2" cellspacing="0" cellpadding="2"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  




!style="background:silver; color:black;" align="center" width="60"|Purpose  
!style="background:silver; color:black;" align="center" width="60"|Purpose  
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
Development of UV resists:
*AZ nLOF
*AZ MiR 701
*AZ 5214E
*AZ 4562
Development of DUV resists:
*KRF M230Y
*KRF M35G
|-
!style="background:silver; color:black;" align="center" width="60"|Developer
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
AZ 726 MIF<br>
(2.38% TMAH in water)
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black"|
Puddle
|-
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black"|
*Chip chuck for chips and 2" wafers
*Non-vacuum chuck for 100 mm and 150 mm wafers
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black"|
1 second rotational agitation at 30 rpm every 15 seconds
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black"|
DI water
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black"|
*Chips (6-60 mm)
*100 mm wafers
*150 mm wafers
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
*All cleanroom approved materials
*Film, or pattern, of all materials except Type IV
|-
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
1
|-
|}
<br clear="all" />
==Developer TMAH UV-lithography==
[[Image:SUSS DEV.JPG|300x300px|right|thumb|Developer: TMAH UV-lithography is located in E-4]]
Developer TMAH UV-lithography was released Q4 2014.
'''[https://www.youtube.com/watch?v=fs9DRH0Eo3k Training video]'''
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=329 LabManager] - '''requires login'''
===[[Specific Process Knowledge/Lithography/Development/Developer TMAH UV-lithography processing|Process Information]]===
*[[Specific Process Knowledge/Lithography/Development/Developer_TMAH_UV-lithography_processing#General_Process_Information|General process information]]
*[[Specific Process Knowledge/Lithography/Development/Developer TMAH UV-lithography_processing#Process recommendations|Process recommendations]]
*[[Specific Process Knowledge/Lithography/Development/Developer TMAH UV-lithography processing#Standard Processes|Standard processes]]
=== Equipment performance and process related parameters ===
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
!style="background:silver; color:black;" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
Line 368: Line 713:
*DUV resists
*DUV resists
|-
|-
!style="background:silver; color:black;" align="center" width="60"|Developer  
!style="background:silver; color:black;" width="60"|Developer  
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black" |
AZ 726 MIF
AZ 726 MIF


(2.38% TMAH in water)
(2.38% TMAH in water)
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="1"|Method
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Puddle
Puddle
|-
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black"|
Vacuum chuck
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Room temperature
Room temperature
|-
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
none
Rotation
|-
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
DI water
DI water
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
* 100 mm wafers
* 100 mm wafers
* 150 mm wafers
* 150 mm wafers
|-
|-
| style="background:LightGrey; color:black"|Allowed materials
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
Silicon, glass, and polymer substrates
Silicon and glass substrates


Film or pattern of all types
Film or pattern of all except Type IV
|-
|-
|style="background:LightGrey; color:black"|Batch
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black"|
1  
1-25
|-  
|-  
|}
|}
<br clear="all" />


<br clear="all" />
{{:Specific Process Knowledge/Lithography/Development/DUV_developer}}

Latest revision as of 13:15, 10 October 2024

The contents on this page, including all images and pictures, was created by DTU Nanolab staff unless otherwise stated.

Feedback to this page: click here

Development Comparison Table

Equipment Developer: SU8 (Wet bench) Developer: E-beam 02 Developer: TMAH Manual 02 Developer: TMAH UV-lithography Developer: TMAH Stepper
Purpose


Development of:

  • SU-8

Development of:

  • ZEP 520A
  • AR-P 6200.xx (CSAR)

Development of:

  • AZ nLOF
  • AZ MiR 701
  • AZ 5214E
  • AZ 4562
  • DUV resists

Development of:

  • AZ nLOF
  • AZ MiR 701
  • AZ 5214E
  • AZ 4562
  • DUV resists

Post-exposure baking

Development of:

  • DUV resists

Post-exposure baking

Developer

mr-Dev 600 (PGMEA)

  • ZED N-50
  • AR-600-546

AZ 726 MIF (2.38% TMAH in water)

AZ 726 MIF (2.38% TMAH in water)

AZ 726 MIF (2.38% TMAH in water)

Method Development

Submersion

Spray/Puddle

Puddle

Puddle

Puddle

Handling
  • Single wafer carrier
  • Chip bucket
  • 100 mm carrier for up to 6 wafers
  • Vacuum chuck for 100 mm & 150 mm substrates
  • Chip chuck for chips & 2" substrates
  • Vacuum chuck for 100 mm & 150 mm substrates
  • Chip chuck for chips & 2" substrates

Vacuum chuck

Vacuum chuck

Process parameters Temperature

Room temperature

Room temperature

Room temperature

Room temperature

Room temperature

Agitation

Magnetic stirrer

Rotation

Rotation

Rotation

Rotation

Rinse

IPA

IPA

DI water

DI water

DI water

Substrates Substrate size
  • Chips
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers
  • Chips (5mm to 2")
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • Chips (5mm to 2")
  • 100 mm wafers
  • 150 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers (may require tool change)
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers (may require tool change)
Allowed materials
  • Silicon and glass substrates
  • Film or pattern of all but Type IV

All cleanroom approved materials

  • All cleanroom approved materials
  • Film or pattern of all types
  • Silicon and glass substrates
  • Film or pattern of all but Type IV
  • Silicon, III-V, and glass substrates
  • Film or pattern of all but Type IV
Batch

1 - 6

1

1

1 - 25

1 - 25



Developer: SU8 (Wet Bench)

The Developer: SU8(Wet Bench)is located in E-4 room.

The SU8-Developer bench is a manually operated wet bench for submersion development of SU-8 photoresist in PGMEA (supplied in the cleanroom as mr-Dev 600). The development process is in two stages; one bath (FIRST) to dissolve the bulk of the resist, and a second, cleaner bath (FINAL) to finish the development. The development time is controlled manually by the user. After development, the substrates are rinsed with IPA in dedicated IPA bath and put for drying in the empty bath.

The user manual, user APV, and contact information can be found in LabManager: Developer: SU8(Wet Bench) - requires login

Process information

Several aspects of the outcome of SU-8 processing are affected by the development process. The lithographic resolution is affected by the time between PEB (post-exposure bake) and development, as the cross-linking process continues in the interface between exposed and unexposed regions even at room temperature. Cracks in the structures is affected by two things; the development time, and how much has previously been developed in the developer bath. Cracking is worse with longer development time, and worst in a new developer bath. The effect of the developer use quickly saturates (5-10 wafers). Finally, the stability of fine structures (high aspect ratio) is affected by the rinse after development, as the lower surface tension of IPA compared to PGMEA reduces pattern collapse during drying.


Development time is strongly dependent on the SU-8 thickness.

  • Minimum development time: 1 min per 20 µm in FIRST


Suggestions:

  • 2-5µm: 2 min. in FIRST; 2 min. in FINAL
  • 40µm: 5 min. in FIRST; 5 min. in FINAL (however, 3 min. in FIRST and 2 min. in FINAL is sufficient)
  • 180-250µm: 15 min. in FIRST; 15 min. in FINAL

Equipment performance and process related parameters

Purpose

Development of:

  • SU-8
Developer

mr-Dev 600

(PGMEA)

Method Development

Submersion

Handling

Single wafer holder

Process parameters Temperature

Room temperature

Agitation

Magnetic stirrer

Rinse

IPA

Substrates Substrate size
  • 100 mm wafers
  • 150 mm wafers, check the liquid level in the baths
  • 200 mm wafer, check the liquid level in the baths
Allowed materials
  • Silicon and glass substrates
  • Film, or pattern, of all materials except Type IV
Batch

1-6


Developer: E-beam 02

Developer: E-beam 02 is located in E-4

Developer: E-beam 02 is a manually operated, single substrate puddle developer. It uses the ZED-N50 or AR 600-50 developers and IPA for rinsing. The substrates are loaded manually one by one into the developer. Developer dispense, puddle time, IPA rinse, and drying is then performed automatically by the equipment.

Training video (for Developer: TMAH Manual, but it is the same model)

The user manual, user APV, and contact information can be found in LabManager - requires login

Process information

All recipes use the following structure:

  1. Pressurize the developer canister
  2. Dispense puddle while rotating substrate slowly
  3. Puddle development while not rotating
  4. Agitate substrate once per 15 seconds by rotating slowly for 1 second
  5. Spin off developer
  6. Clean substrate with IPA
  7. Dry substrate and chamber with nitrogen

Multi-puddle recipes repeat steps 2-5 for the given number of puddles.


Process recipes
N50 recipes have the letter "N" in them. AR-600-50 recipes have the letter "A" in them. The number is the development time in seconds:

  • 01 Rinse
  • 02 N 15
  • 03 N 30
  • 04 N 60
  • 05 N 90
  • 06 N 120
  • 07 N 180
  • 08 N 300
  • 09 N 600
  • 10 N 2x60
  • 11 N 5x60
  • 12 A 15
  • 13 A 30
  • 14 A 60
  • 15 A 90
  • 16 A 120
  • 17 A 180
  • 18 A 300
  • 19 A 600
  • 20 A 2x60
  • 21 A 5x60

Equipment performance and process related parameters

Purpose

Development of:

  • CSAR
  • ZEP520A
Developer
  • AR 600-50
  • ZED N-50
Method Development

Puddle

Handling
  • Chip chuck for chips
  • Non-vacuum chuck for 2" wafers
  • Non-vacuum chuck for 100 mm and 150 mm wafers
  • Non-vacuum chuck for 200 mm wafers
Process parameters Temperature

Room temperature

Agitation

1 second rotational agitation at 30 rpm every 15 seconds

Rinse

IPA

Substrates Substrate size
  • Chips
  • 2" wafers
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers
Allowed materials
  • All cleanroom approved materials
  • Film, or pattern, of all materials except Type IV
Batch size

1


Developer: TMAH Manual 02

Developer: TMAH Manual 02 is located in E-4

Developer: TMAH Manual 02 is a manually operated, single substrate or chip puddle developer. It uses the TMAH based AZ 726 MIF developer (2.38 % TMAH in water with a small amount of wetting agent). The substrates or chips are loaded manually one by one into the developer. Developer dispense, puddle time, water rinse, and drying is performed automatically by the equipment.


Training video


The user manual, user APV, and contact information can be found in LabManager - requires login

Process information

All recipes use the following structure:

  1. Pressurize the TMAH canister
  2. Dispense puddle while rotating substrate slowly
  3. Puddle development while not rotating
  4. Agitate substrate once per 15 seconds by rotating slowly for 1 second
  5. Spin off developer
  6. Clean substrate and chamber with DI water
  7. Dry substrate and chamber with nitrogen

Multi-puddle recipes repeat steps 2-5 for the given number of puddles.


Process recipes
SP: Single-puddle
MP: Multi-puddle

  • 01 Rinse
  • 02 SP 15
  • 03 SP 30
  • 04 SP 60
  • 05 SP 90
  • 06 SP 120
  • 07 SP 300
  • 08 MP 2x60
  • 09 MP 5x60
  • 91 SP test
  • 92 MP test

Equipment performance and process related parameters

Purpose

Development of UV resists:

  • AZ nLOF
  • AZ MiR 701
  • AZ 5214E
  • AZ 4562

Development of DUV resists:

  • KRF M230Y
  • KRF M35G
Developer

AZ 726 MIF
(2.38% TMAH in water)

Method Development

Puddle

Handling
  • Chip chuck for chips and 2" wafers
  • Non-vacuum chuck for 100 mm and 150 mm wafers
Process parameters Temperature

Room temperature

Agitation

1 second rotational agitation at 30 rpm every 15 seconds

Rinse

DI water

Substrates Substrate size
  • Chips (6-60 mm)
  • 100 mm wafers
  • 150 mm wafers
Allowed materials
  • All cleanroom approved materials
  • Film, or pattern, of all materials except Type IV
Batch size

1


Developer TMAH UV-lithography

Developer: TMAH UV-lithography is located in E-4

Developer TMAH UV-lithography was released Q4 2014.


Training video


The user manual, user APV, and contact information can be found in LabManager - requires login

Process Information

Equipment performance and process related parameters

Purpose

Development of

  • AZ nLOF
  • AZ MiR 701
  • AZ 5214E
  • AZ 4562
  • DUV resists
Developer

AZ 726 MIF

(2.38% TMAH in water)

Method Development

Puddle

Handling

Vacuum chuck

Process parameters Temperature

Room temperature

Agitation

Rotation

Rinse

DI water

Substrates Substrate size
  • 100 mm wafers
  • 150 mm wafers
Allowed materials

Silicon and glass substrates

Film or pattern of all except Type IV

Batch

1-25


Developer: TMAH Stepper

The Developer-TMAH-Stepper is placed in F-3

This developer is dedicated for development of DUV resists. The developer is fully automatic and can run up to 25 substrates in a batch 4", 6", and 8" size (8" requires tool change). The machine is equipped with 1 developer line, in our case 2,38% TMAH in water (AZ 726 MIF), 1 topside rinse line with water, 1 backside rinse line with water and 1 N2 line for drying.


The user manual and contact information can be found in LabManager - requires login


Process information

The SEM picture of 250 nm pillars and lines. Exposure dose is 140 J/m2.

The development process will be performed by the customer together with the Photolith group of DTU Nanolab. In case you would like to do DUV lithography please contact Lithography team, who will consult you and run your wafers together with you.

Here you can find a chart‎ demonstrating a dependence between 250 nm line width/pillars diameter and exposure dose.

Standard processes

Post-exposure bake sequences:

  • (1000) DCH PEB 130C 60s 60s baking at 130°C; 20s cooling
  • (1001) DCH PEB 130C 90s 90s baking at 130°C; 20s cooling

Development sequences:

  • (1004) DCH DEV 60s 60s single puddle development

Combined PEB and development sequences:

  • (1002) DCH PEB_60s and DEV_60s 60s baking at 130°C followed by 60s single puddle development
  • (1003) DCH PEB_90s and DEV_60s 90s baking at 130°C followed by 60s single puddle development

The standard developer process consists of:

  • pre-wetting with water (2.5s @ 1000rpm)
  • developer dispense (2.5s @ 40rpm, corresponding to ~9ml)
  • development (60s @ 0rpm)
  • water rinse with BSR (5s @ 3000rpm)
  • nitrogen drying (7s @ 4000rpm)

and has a cycle time of ~2 minutes


Equipment performance and process related parameters

Purpose

Development of DUV resist: KRF M230Y and KRF M35G

Developer

2,38% water based TMAH

Process parameters Spin speed

10 - 5000 rpm

Spin acceleration

100 - 10000 rpm/s

Hotplate temperature

130°C for post exposure baking

Substrates Substrate size
  • 100 mm wafers
  • 150 mm wafers
  • 200 mm wafers (requires tool change)
Allowed materials
  • Any standard cleanroom material
Batch

1 - 25