Specific Process Knowledge/Characterization/XRD/XRD SmartLab: Difference between revisions
(44 intermediate revisions by 3 users not shown) | |||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Characterization/XRD/XRD_SmartLab click here]''' | |||
<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b><br> | |||
All images and photos on this page belongs to <b>DTU Nanolab</b></i> | |||
= XRD SmartLab = | = XRD SmartLab = | ||
Line 4: | Line 10: | ||
The Rigaku SmartLab is an advanced XRD for measuring on thin films. All thin films can be measured without fixating the sample, as the system has a so called In-Plane arm. | The Rigaku SmartLab is an advanced XRD for measuring on thin films. All thin films can be measured without fixating the sample, as the system has a so called In-Plane arm. | ||
[[image:XRD_SmartLab.jpg| | [[image:XRD_SmartLab.jpg|400x400px|right|thumb|The XRD SmartLab located in cleanroom F-2]] | ||
'''The user manual(s), user APV(s), technical information, and contact information can be found in LabManager:''' | '''The user manual(s), user APV(s), technical information, and contact information can be found in LabManager:''' | ||
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=428 XRD SmartLab in LabManager] | [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=428 XRD SmartLab in LabManager] - requires login | ||
Various measurement types including X-Ray reflectivity, Rocking curve, Theta-2theta, and Pole figures are described here: | |||
[http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Characterization/XRD/Process_Info Process information] | [http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Characterization/XRD/Process_Info Process information] | ||
The measurement settings and results of the pre-acceptance test are described in this document, also found on the Lab Manager: | |||
*[https://labmanager.dtu.dk/view_binary.php?fileId=5413| (FAT) Factory Acceptance Test] - requires login | |||
The same measurement were completed as part of the acceptance, but no report was generated. In addition the inspection certificate is available here: | |||
*[https://labmanager.dtu.dk/view_binary.php?fileId=5414| (SAT) Site Acceptance Test] - requires login | |||
==Software for analysis== | ==Software for analysis== | ||
The | Please see the Data Analysis section at the main [[Specific Process Knowledge/Characterization/XRD|XRD page]]. | ||
==Characterization of thin films using X-ray reflectivity (XRR)== | |||
Implementing the XRR method the user can calculate thickness, density, and roughness of the deposited material. The XRR is also widely employed for multilayer stack analysis. | |||
Here are some results available: | |||
* Characterization of [[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Aluminium/Al_Ebeam_evaporation_in_Temescal|e-beam deposited Al thin films]]. | |||
* Characterization of [[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Aluminium/Al_Sputtering_in_Cluster_Lesker_PC3#X-ray_reflectivity_analysis|DC sputtered Al thin films]]. | |||
* Characterization of [[Specific_Process_Knowledge/Characterization/XRD/XRD_SmartLab/ALD_deposited_alumina_and_titania_XRR#X-ray_reflectivity_results|ALD deposited Al<sub>2</sub>O<sub>3</sub> and TiO<sub>2</sub> ultrathin layers]]. | |||
* Characterization of [[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_CrSi#X-ray_Reflectivity_Analysis|Sputtered deposited CrSi bilayer]]. | |||
* Characterization of [[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_MgO#X-Ray_Reflectivity|Sputtered deposited MgO thin films]]. | |||
* Characterization of [[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Scandium/Sc_Sputtering_in_Cluster_Lesker_PC3#X-ray_Reflectivity_(XRR)|Sputtered deposited Sc thin films]]. | |||
* Characterization of [[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Scandium_Nitride/ScN_Reactive_Sputtering_in_Cluster_Lesker_PC3#X-ray_Reflectivity_(XRR)|Sputtered deposited ScN thin films]]. | |||
<!-- * Characterization of [[Specific_Process_Knowledge/Characterization/XRD/XRD_SmartLab/ALD_deposited_alumina_and_titania_XRR_and_SE_comparison|ALD deposited Al<sub>2</sub>O<sub>3</sub> and TiO<sub>2</sub> ultrathin layers]].--> | |||
==Grazing Incidence X-ray Diffraction XRD (GiXRD)== | |||
* Evaluation of [[Specific Process Knowledge/Characterization/XRD/XRD SmartLab/Instrumental broading in GiXRD|Instrumental broading in GiXRD]]. | |||
==θ/2θ X-ray Diffraction== | |||
* Evaluation of [[Specific Process Knowledge/Characterization/XRD/XRD SmartLab/Instrumental broading in T2T|Instrumental broadening in symmetrical θ/2θ measurements]]. | |||
==Equipment performance and process related parameters== | ==Equipment performance and process related parameters== | ||
Line 25: | Line 72: | ||
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment | !colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment | ||
|style="background:WhiteSmoke; color:black"|<b>XRD SmartLab</b> | |style="background:WhiteSmoke; color:black"|<b>XRD SmartLab</b> | ||
|- | |- | ||
!style="background:silver; color:black;" align="center" width="60"|Purpose | !style="background:silver; color:black;" align="center" width="60"|Purpose | ||
Line 42: | Line 88: | ||
*Roughness | *Roughness | ||
*Density | *Density | ||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="6"|X-ray generator | !style="background:silver; color:black" align="center" valign="center" rowspan="6"|X-ray generator | ||
Line 52: | Line 95: | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
3 kW | 3 kW | ||
|- | |- | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
Line 59: | Line 100: | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
20 to 45 kV | 20 to 45 kV | ||
|- | |- | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
Line 66: | Line 105: | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
2 to 60 mA | 2 to 60 mA | ||
|- | |- | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
Type | Type | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
Sealed tube | Sealed tube | ||
Line 78: | Line 113: | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
Target | Target | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
Cu | Cu | ||
Line 87: | Line 120: | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
0.4 mm x 8 mm (Line/Point) | 0.4 mm x 8 mm (Line/Point) | ||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan=" | !style="background:silver; color:black" align="center" valign="center" rowspan="4"|Goniometer | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
Scanning mode | Scanning mode | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
incident / receiver coupled or independent | incident / receiver coupled or independent | ||
|- | |- | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
Line 102: | Line 131: | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
300 mm | 300 mm | ||
|- | |- | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
Line 109: | Line 136: | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
0.0001° (0.36") | 0.0001° (0.36") | ||
|- | |- | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
Line 120: | Line 145: | ||
*X,Y:±50 mm for a 100 mm wafer | *X,Y:±50 mm for a 100 mm wafer | ||
*Rx,Ry:-5~+5° | *Rx,Ry:-5~+5° | ||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Optics | !style="background:silver; color:black" align="center" valign="center" rowspan="2"|Optics | ||
|style="background:LightGrey; color:black"|Incident side | |style="background:LightGrey; color:black"|Incident side | ||
Line 139: | Line 155: | ||
*Soller slit | *Soller slit | ||
*Variable divergence slit | *Variable divergence slit | ||
|- | |- | ||
|style="background:LightGrey; color:black"|Receiver side | |style="background:LightGrey; color:black"|Receiver side | ||
Line 151: | Line 162: | ||
*Parallel slit analysers (PSA) | *Parallel slit analysers (PSA) | ||
*Ge(220)x2 analyser | *Ge(220)x2 analyser | ||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates | !style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates | ||
|style="background:LightGrey; color:black"|Substrate size | |style="background:LightGrey; color:black"|Substrate size | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
up to 150 mm wafers | up to 150 mm wafers; thickness up to 21 mm | ||
|- | |- | ||
| style="background:LightGrey; color:black"|Allowed materials | | style="background:LightGrey; color:black"|Allowed materials | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
All materials | All materials allowed in the cleanroom | ||
|- | |- | ||
|} | |} | ||
<br clear="all" /> | <br clear="all" /> |
Latest revision as of 09:39, 31 July 2024
Feedback to this page: click here
Unless otherwise stated, this page is written by DTU Nanolab internal
All images and photos on this page belongs to DTU Nanolab
XRD SmartLab
The Rigaku SmartLab is an advanced XRD for measuring on thin films. All thin films can be measured without fixating the sample, as the system has a so called In-Plane arm.

The user manual(s), user APV(s), technical information, and contact information can be found in LabManager:
XRD SmartLab in LabManager - requires login
Various measurement types including X-Ray reflectivity, Rocking curve, Theta-2theta, and Pole figures are described here:
The measurement settings and results of the pre-acceptance test are described in this document, also found on the Lab Manager:
- (FAT) Factory Acceptance Test - requires login
The same measurement were completed as part of the acceptance, but no report was generated. In addition the inspection certificate is available here:
- (SAT) Site Acceptance Test - requires login
Software for analysis
Please see the Data Analysis section at the main XRD page.
Characterization of thin films using X-ray reflectivity (XRR)
Implementing the XRR method the user can calculate thickness, density, and roughness of the deposited material. The XRR is also widely employed for multilayer stack analysis.
Here are some results available:
- Characterization of e-beam deposited Al thin films.
- Characterization of DC sputtered Al thin films.
- Characterization of ALD deposited Al2O3 and TiO2 ultrathin layers.
- Characterization of Sputtered deposited CrSi bilayer.
- Characterization of Sputtered deposited MgO thin films.
- Characterization of Sputtered deposited Sc thin films.
- Characterization of Sputtered deposited ScN thin films.
Grazing Incidence X-ray Diffraction XRD (GiXRD)
- Evaluation of Instrumental broading in GiXRD.
θ/2θ X-ray Diffraction
- Evaluation of Instrumental broadening in symmetrical θ/2θ measurements.
Equipment | XRD SmartLab | |
---|---|---|
Purpose | Crystal structure analysis and thin film thickness measurement |
|
X-ray generator |
Maximum rated output |
3 kW |
Rated tube voltage |
20 to 45 kV | |
Rated tube current |
2 to 60 mA | |
Type |
Sealed tube | |
Target |
Cu | |
Focus size |
0.4 mm x 8 mm (Line/Point) | |
Goniometer |
Scanning mode |
incident / receiver coupled or independent |
Goniomenter radius |
300 mm | |
Minimum step size |
0.0001° (0.36") | |
Sample stage |
| |
Optics | Incident side |
|
Receiver side |
| |
Substrates | Substrate size |
up to 150 mm wafers; thickness up to 21 mm |
Allowed materials |
All materials allowed in the cleanroom |