=Etching of very thin layer of SiO2=
=Etching of very thin layer of SiO2=
Pegasus 3 is not meant to be used as an SiO2 etcher. Please do not develop nice SiO2 recipes on this machine. Often SIO2 etch recipes are very polymerizing and that can disturb the chamber conditions for the silicon etching recipes.
Pegasus 3 is not meant to be used as an SiO2 etcher. Please do not develop SiO2 recipes on this machine. Often SiO2 etch recipes are very polymerizing and that can disturb the chamber conditions for the silicon etching recipes.


The recipe developed here is only for etching through a very thin SiO2 layer and does not have a high selectivity to silicon to avoid the recipe to become too polymerizing. It is also not very uniform over the wafer, so when it is used for etching down to silicon it will also etch a lot in the silicon and in areas more than other.
The recipe developed here is only for etching through a very thin SiO2 layer and does not have a high selectivity to silicon to avoid the recipe to become too polymerizing. It is also not very uniform over the wafer, so when it is used for etching down to silicon it will also etch a lot in the silicon and in areas more than other.
Line 6: Line 6:
==Test work done==
==Test work done==
{{CC-bghe2}} <br>
{{CC-bghe2}} <br>
The tests were done on 6" wafers. Siliocn wafers with 1µm thermal SiO2 and maskless. Measurements were done on the ellipsometer before at after the etch to map the etch rate.
The tests were done on 6" wafers. Silicon wafers with 1µm thermal SiO2 and mask less. Measurements were done on the ellipsometer before at after the etch to map the etch rate.


{| class="wikitable"
{| class="wikitable"
|+ Tests with SiO2 etch
|+ Tests with SiO2 etch
|-
|-
! Wafer number !! C4F8 !! SF6 flow !! Ar !! Coil power !! Platen power !! Presure
! Wafer number !! C4F8 !! SF6 flow !! Ar !! Platen power !! Pressure || SiO2 Uniformity results || SiO2 Center Etch rate ||Si Center Etch rate || Si Uniformity
|-
|-
| Y34 || Example || Example || Example || Example || Example || Example
| Y34 || 50 sccm|| 50 sccm|| 0 sccm|| 100 W || 80 mTorr || &plusmn;23.3% || 36.0 nm/min (highest)|| ||
|-
|-
| Y35 || Example || Example || Example || Example || Example || Example
| Y35 || 25 sccm|| 75 sccm|| 0 sccm|| 100 W || 80 mTorr || &plusmn;20.8% || 41.3 nm/min (highest) || ||
|-
|-
| Y36 || Example || Example || Example || Example || Example || Example
| Y36 || 25 sccm|| 75 sccm|| 0 sccm|| 100 W || 10 mTorr || &plusmn;22.1% || 36.2 nm/min (lowest) || ||
|-
|-
| Y37 || Example || Example || Example || Example || Example || Example
| Y37 ||25 sccm|| 75 sccm|| 0 sccm|| 100 W || 40 mTorr || &plusmn;24.6% || 24.4 nm/min (lowest) || ||
|-
|-
| Y38 || Example || Example || Example || Example || Example || Example
| Y38 || 25 sccm|| 75 sccm|| 0 sccm|| 100 W || 60 mTorr || &plusmn; 8.1% || 34.0 nm/min (highest in center and at edge) || 141.4@15s, 137.5@2min || &plusmn; 13.9%@15s, &plusmn; 16.5%@2min
|-
|-
| Y39 || Example || Example || Example || Example || Example || Example
| Y39 || 50 sccm|| 150 sccm|| 0 sccm|| 100 W || 10 mTorr || &plusmn;25.0% || 34.8 nm/min (lowest)|| ||
|-
|-
| Y40 || Example || Example || Example || Example || Example || Example
| Y40 || 8.33 sccm|| 50 sccm|| 100 sccm|| 100 W || 10 mTorr || &plusmn;15.1% || 35.8 n/min (lowest)|| 70.8@15s, 107.5@5min || &plusmn; 17.6%@15s, &plusmn; 11.1%@4min
|}
 
{| class="wikitable"
|+ Etch uniformity
|-
! SiO2 etch rate uniformity !! SiO2 etch rate uniformity normalized to center!! Si Etch rate uniformity
|-
| [[File:Peg3 SiO2 uniformity Y34 to Y40.jpg]] || [[File:Peg3 SiO2 uniformity normalized Y34 to Y40.jpg]] || valign="top"| [[File:Peg3 Si etch uniformity Y38 and Y40.jpg]]
|}
|}
[[File:Peg3 SIO2 uniformity - Contour Plot 5.jpg|400px]]

Latest revision as of 17:02, 29 January 2024

Etching of very thin layer of SiO2

Pegasus 3 is not meant to be used as an SiO2 etcher. Please do not develop SiO2 recipes on this machine. Often SiO2 etch recipes are very polymerizing and that can disturb the chamber conditions for the silicon etching recipes.

The recipe developed here is only for etching through a very thin SiO2 layer and does not have a high selectivity to silicon to avoid the recipe to become too polymerizing. It is also not very uniform over the wafer, so when it is used for etching down to silicon it will also etch a lot in the silicon and in areas more than other.

Test work done

Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
The tests were done on 6" wafers. Silicon wafers with 1µm thermal SiO2 and mask less. Measurements were done on the ellipsometer before at after the etch to map the etch rate.

Tests with SiO2 etch
Wafer number C4F8 SF6 flow Ar Platen power Pressure SiO2 Uniformity results SiO2 Center Etch rate Si Center Etch rate Si Uniformity
Y34 50 sccm 50 sccm 0 sccm 100 W 80 mTorr ±23.3% 36.0 nm/min (highest)
Y35 25 sccm 75 sccm 0 sccm 100 W 80 mTorr ±20.8% 41.3 nm/min (highest)
Y36 25 sccm 75 sccm 0 sccm 100 W 10 mTorr ±22.1% 36.2 nm/min (lowest)
Y37 25 sccm 75 sccm 0 sccm 100 W 40 mTorr ±24.6% 24.4 nm/min (lowest)
Y38 25 sccm 75 sccm 0 sccm 100 W 60 mTorr ± 8.1% 34.0 nm/min (highest in center and at edge) 141.4@15s, 137.5@2min ± 13.9%@15s, ± 16.5%@2min
Y39 50 sccm 150 sccm 0 sccm 100 W 10 mTorr ±25.0% 34.8 nm/min (lowest)
Y40 8.33 sccm 50 sccm 100 sccm 100 W 10 mTorr ±15.1% 35.8 n/min (lowest) 70.8@15s, 107.5@5min ± 17.6%@15s, ± 11.1%@4min
Etch uniformity
SiO2 etch rate uniformity SiO2 etch rate uniformity normalized to center Si Etch rate uniformity