Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Nickel: Difference between revisions

From LabAdviser
Reet (talk | contribs)
removed physimeca
Reet (talk | contribs)
(11 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Nickel click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Nickel click here]'''
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''
'''All links to Labmanager Including APV and QC requires login.'''


== Nickel deposition ==
== Nickel deposition ==
Nickel can be deposited by e-beam evaporation, sputtering or electroplating. In the chart below you can compare the different deposition equipment.
Nickel can be deposited by e-beam evaporation or sputtering at DTU Nanolab. For electroplating you will have to contact other institutes at DTU, e.g., DTU Mechanical Engineering.  


*[[/Electroplating of nickel|Electroplating of nickel]]
Some process information is available here for e-beam evaporated films:
<!--*[[/Electroplating of nickel|Electroplating of nickel]]-->
*[[/Stress Wordentec Ni films|Stress in Wordentec Ni films: study here]].
*[[/Stress Wordentec Ni films|Stress in Wordentec Ni films: study here]].


 
In the chart below you can compare the different deposition equipment:


{| border="1" cellspacing="0" cellpadding="3"  
{| border="1" cellspacing="0" cellpadding="3"  
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!  
!  
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|Temescal]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]] and [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]])
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]])
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]])
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]])
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]])
! Electroplating ([[Specific Process Knowledge/Thin film deposition/Electroplating-Ni|Electroplating-Ni]])
|-  
|-  


Line 26: Line 30:
|Sputter deposition of Nickel
|Sputter deposition of Nickel
|Sputter deposition of Nickel
|Sputter deposition of Nickel
|Electroplating of Nickel
|-
|-


Line 32: Line 35:
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
! Pre-clean
! Pre-clean
|Ar ion bombardment
|Ar ion etch (only in E-beam evaporator Temescal)
|
|
|RF Ar clean
|RF Ar clean
|RF Ar clean
|RF Ar clean
|None
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
Line 45: Line 47:
|10 Å to 5000 Å **
|10 Å to 5000 Å **
|10 Å to 5000 Å **
|10 Å to 5000 Å **
|~ 20 µm to ~ 1000 µm
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"


! Deposition rate
! Deposition rate
|2-10 Å/s
|1-10 Å/s
|10-15 Å/s
|1-10 Å/s
|Depends on process parameters, about 1 Å/s  
|Depends on process parameters, about 1 Å/s  
|Depends on process parameters, at least ~ 4 Å/s, see conditions [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|here]]
|Depends on process parameters, at least ~ 4 Å/s, see conditions [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|here]]
|~ 10-250 Å/s


|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
Line 74: Line 74:
*Up to 10x4" or 6" wafers
*Up to 10x4" or 6" wafers
*Many smaller pieces
*Many smaller pieces
|
*1x2" wafer or
*1x4" wafer or
*1x6" wafer


|-
|-
Line 85: Line 81:


|
|
* Silicon
*Almost any that does not degas at your intended substrate temperature. See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet]
*Silicon oxide
*Silicon (oxy)nitride
*Photoresist
*PMMA
*Mylar
*Metals
*See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet]
|
|
* Silicon
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=167 cross-contamination sheet].
* Silicon oxide
* Silicon nitride
* Silicon (oxy)nitride
* Photoresist
* PMMA
* Mylar
* SU-8
|
|
* Almost any that do not outgas.
* Almost any that do not degas.
|
|
*Almost any that do not outgas. Check the cross-contamination sheet in Labmanager.
*Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3]
|
 
Base materials:<br>
*Silicon
*Polymers with Tg > 75°C
*Metals (bulk)
*Cross-linked or hard baked resists supported by one of the above mentioned materials
Seed metals:<br>
* NiV (75 - 100 nm recommended)
* Ti (~5 nm) + Au (75-100 nm recommended)
* Cr (~5 nm) + Au (75-100 nm recommended)
* TiW
* Cr
|-
|-
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
! Comment
! Comment
|  
|
|
|
*[[/Stress Wordentec Ni films|Stress in Wordentec Ni films: study here]].  
*[[/Stress Wordentec Ni films|Stress in Wordentec Ni films: study here]].  
|
|
|
*May use high-strength magnet for deposition.  
*May use high-strength magnet for deposition.  
|
|
*May use high-strength magnet for deposition
*May use high-strength magnet for deposition
|
*Sample must be compatible with plating bath (pH = 3,65 and T = 52°C). Seed metal necessary.
|-
|-


Line 140: Line 108:


'''**''' ''To deposit a cumulative thickness above 200 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine''
'''**''' ''To deposit a cumulative thickness above 200 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine''


==Quality control of e-beam evaporated Ni films==
==Quality control of e-beam evaporated Ni films==
Line 148: Line 115:
|-
|-
|
|
*[http://labmanager.dtu.dk/d4Show.php?id=3736&mach=167 QC procedure for Wordentec]<br>
Nickel deposition is tested occasionally, around 1-2 times per year. LabManager links require login.
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=167 The newest QC data for Wordentec]<br>
*[http://labmanager.dtu.dk/d4Show.php?id=3736&mach=167 QC procedure for Wordentec in LabManager]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=167 The newest QC data for Wordentec in LabManager]<br>


{| {{table}}
{| {{table}}
Line 190: Line 158:
|-
|-
|
|
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=429 QC procedure for the Temescal]<br>
Nickel deposition is tested occasionally, around 1 time per year. LabManager links require login.
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=429 The newest QC data for the Temescal]<br>
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=429 QC procedure for the Temescal in LabManager]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=429 The newest QC data for the Temescal in LabManager]<br>


{| {{table}}
{| {{table}}
Line 228: Line 197:
|}
|}
Thickness is measured in 5 points with a stylus profiler. <br>
Thickness is measured in 5 points with a stylus profiler. <br>
Additionally we examine the newly deposited films for particles using the particle scanner (if available, otherwise we use the Jenatech microscope in darkfield mode) and we monitor the sheet resistance of the Ti/Au films.
|}
|}

Revision as of 13:11, 22 January 2024

Feedback to this page: click here

Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.

All links to Labmanager Including APV and QC requires login.

Nickel deposition

Nickel can be deposited by e-beam evaporation or sputtering at DTU Nanolab. For electroplating you will have to contact other institutes at DTU, e.g., DTU Mechanical Engineering.

Some process information is available here for e-beam evaporated films:

In the chart below you can compare the different deposition equipment:

E-beam evaporation (E-beam evaporator (Temescal) and E-beam evaporator (10-pockets)) E-beam evaporation (Wordentec) Sputter deposition (Lesker) Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3))
General description E-beam deposition of Nickel E-beam deposition of Nickel Sputter deposition of Nickel Sputter deposition of Nickel
Pre-clean Ar ion etch (only in E-beam evaporator Temescal) RF Ar clean RF Ar clean
Layer thickness 10 Å to 1 µm * 10 Å to 1 µm * 10 Å to 5000 Å ** 10 Å to 5000 Å **
Deposition rate 1-10 Å/s 1-10 Å/s Depends on process parameters, about 1 Å/s Depends on process parameters, at least ~ 4 Å/s, see conditions here
Batch size
  • Up to 4x6" wafers
  • Up to 3x8" wafers (ask for holder)
  • Many smaller pieces
  • 24x2" wafers or
  • 6x4" wafers or
  • 6x6" wafers
  • Pieces or
  • 1x4" wafer or
  • 1x6" wafer
  • Up to 10x4" or 6" wafers
  • Many smaller pieces
Allowed materials

Almost any that does not degas. See the cross-contamination sheet.

  • Almost any that do not degas.
  • Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for PC1 and PC3
Comment
  • May use high-strength magnet for deposition.
  • May use high-strength magnet for deposition

* To deposit a cumulative thickness above 600 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine


** To deposit a cumulative thickness above 200 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine

Quality control of e-beam evaporated Ni films

Quality control (QC) for Wordentec

Nickel deposition is tested occasionally, around 1-2 times per year. LabManager links require login.

QC Recipe: Process 5
Deposition rate 10 Å/s
Thickness 100 nm
Pressure Below 4*10-6 mbar
QC limits Wordentec
Measured average thickness (Å) ± 10 %
Lowest accepted deposition rate (Å/s) 6 Å/s

Thickness is measured in 5 points with a stylus profiler.


Quality control (QC) for the Temescal

Nickel deposition is tested occasionally, around 1 time per year. LabManager links require login.

QC Recipe: Standard recipes/Ni
Deposition rate 10 Å/s
Thickness 100 nm
Pressure Below 1*10-6 mbar
QC limits Temescal
Deposition rate deviation ± 20 %
Measured average thickness ± 10 %
Thickness deviation across a 4" wafer ± 5 %

Thickness is measured in 5 points with a stylus profiler.