Specific Process Knowledge/Thin film deposition/Deposition of Nickel: Difference between revisions
| (21 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Nickel click here]''' | ||
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.''' | |||
'''All links to Labmanager Including APV and QC requires login.''' | |||
== Nickel deposition == | == Nickel deposition == | ||
Nickel can be deposited by e-beam evaporation or electroplating. | Nickel can be deposited by e-beam evaporation or sputtering at DTU Nanolab. For electroplating you will have to contact other institutes at DTU, e.g., DTU Mechanical Engineering. | ||
*[[/Electroplating of nickel|Electroplating of nickel]] | Some process information is available here for e-beam evaporated films: | ||
<!--*[[/Electroplating of nickel|Electroplating of nickel]]--> | |||
*[[/Stress Wordentec Ni films|Stress in Wordentec Ni films: study here]]. | *[[/Stress Wordentec Ni films|Stress in Wordentec Ni films: study here]]. | ||
In the chart below you can compare the different deposition equipment: | |||
{| border="1" cellspacing="0" cellpadding="3" | {| border="1" cellspacing="0" cellpadding="3" | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
! | ! | ||
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|Temescal]]) | ! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]] and [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]]) | ||
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]]) | ! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]]) | ||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]]) | ! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]]) | ||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster- | ! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]]) | ||
|- | |- | ||
| Line 23: | Line 26: | ||
! General description | ! General description | ||
|E-beam deposition of Nickel | |E-beam deposition of Nickel | ||
|E-beam deposition of Nickel | |E-beam deposition of Nickel | ||
|Sputter deposition of Nickel | |Sputter deposition of Nickel | ||
|Sputter deposition of Nickel | |Sputter deposition of Nickel | ||
|- | |- | ||
| Line 34: | Line 35: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Pre-clean | ! Pre-clean | ||
|Ar ion | |Ar ion etch (only in E-beam evaporator Temescal) | ||
| | | | ||
|RF Ar clean | |RF Ar clean | ||
|RF Ar clean | |RF Ar clean | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Layer thickness | ! Layer thickness | ||
| | |10 Å to 1 µm * | ||
| | |10 Å to 1 µm * | ||
| | |10 Å to 5000 Å ** | ||
|10 Å to 5000 Å ** | |||
| | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Deposition rate | ! Deposition rate | ||
| | |1-10 Å/s | ||
|1-10 Å/s | |||
|1 | |Depends on process parameters, about 1 Å/s | ||
|Depends on process parameters | |Depends on process parameters, at least ~ 4 Å/s, see conditions [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|here]] | ||
|Depends on process parameters | |||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
| Line 72: | Line 67: | ||
*6x4" wafers or | *6x4" wafers or | ||
*6x6" wafers | *6x6" wafers | ||
| | | | ||
* Pieces or | * Pieces or | ||
| Line 83: | Line 74: | ||
*Up to 10x4" or 6" wafers | *Up to 10x4" or 6" wafers | ||
*Many smaller pieces | *Many smaller pieces | ||
|- | |- | ||
| Line 94: | Line 81: | ||
| | | | ||
* | *Almost any that does not degas at your intended substrate temperature. See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet] | ||
| | | | ||
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=167 cross-contamination sheet]. | |||
| | | | ||
* | * Almost any that do not degas. | ||
| | | | ||
* | *Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3] | ||
|- | |- | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Comment | ! Comment | ||
| | | | ||
| | | | ||
*[[/Stress Wordentec Ni films|Stress in Wordentec Ni films: study here]]. | *[[/Stress Wordentec Ni films|Stress in Wordentec Ni films: study here]]. | ||
| | | | ||
*May use high-strength magnet for deposition. | |||
| | | | ||
*May use high-strength magnet for deposition | |||
|- | |- | ||
|} | |} | ||
'''*''' ''To deposit | '''*''' ''To deposit a cumulative thickness above 600 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine'' | ||
'''**''' ''To deposit a cumulative thickness above 200 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine'' | |||
==Quality control of e-beam evaporated Ni films== | |||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality control (QC) for Wordentec''' | |||
|- | |||
| | |||
Nickel deposition is tested occasionally, around 1-2 times per year. LabManager links require login. | |||
*[http://labmanager.dtu.dk/d4Show.php?id=3736&mach=167 QC procedure for Wordentec in LabManager]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=167 The newest QC data for Wordentec in LabManager]<br> | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:300px" | |||
! QC Recipe: | |||
! Process 5 | |||
|- | |||
|Deposition rate | |||
|10 Å/s | |||
|- | |||
|Thickness | |||
|100 nm | |||
|- | |||
|Pressure | |||
|Below 4*10<sup>-6</sup> mbar | |||
|- | |||
|} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:440px" | |||
!QC limits | |||
!Wordentec | |||
|- | |||
|Measured average thickness (Å) | |||
|± 10 % | |||
|- | |||
|Lowest accepted deposition rate (Å/s) | |||
|6 Å/s | |||
|- | |||
|} | |||
|- | |||
|} | |||
Thickness is measured in 5 points with a stylus profiler. | |||
|} | |||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality control (QC) for the Temescal''' | |||
|- | |||
| | |||
Nickel deposition is tested occasionally, around 1 time per year. LabManager links require login. | |||
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=429 QC procedure for the Temescal in LabManager]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=429 The newest QC data for the Temescal in LabManager]<br> | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:400px" | |||
! QC Recipe: | |||
! Standard recipes/Ni | |||
|- | |||
|Deposition rate | |||
|10 Å/s | |||
|- | |||
|Thickness | |||
|100 nm | |||
|- | |||
|Pressure | |||
|Below 1*10<sup>-6</sup> mbar | |||
|- | |||
|} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:440px" | |||
!QC limits | |||
!Temescal | |||
|- | |||
|Deposition rate deviation | |||
|± 20 % | |||
|- | |||
|Measured average thickness | |||
|± 10 % | |||
|- | |||
|Thickness deviation across a 4" wafer | |||
|± 5 % | |||
|- | |||
|} | |||
|- | |||
|} | |||
Thickness is measured in 5 points with a stylus profiler. <br> | |||
|} | |||
Revision as of 13:11, 22 January 2024
Feedback to this page: click here
Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.
All links to Labmanager Including APV and QC requires login.
Nickel deposition
Nickel can be deposited by e-beam evaporation or sputtering at DTU Nanolab. For electroplating you will have to contact other institutes at DTU, e.g., DTU Mechanical Engineering.
Some process information is available here for e-beam evaporated films:
In the chart below you can compare the different deposition equipment:
| E-beam evaporation (E-beam evaporator (Temescal) and E-beam evaporator (10-pockets)) | E-beam evaporation (Wordentec) | Sputter deposition (Lesker) | Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) | |
|---|---|---|---|---|
| General description | E-beam deposition of Nickel | E-beam deposition of Nickel | Sputter deposition of Nickel | Sputter deposition of Nickel |
| Pre-clean | Ar ion etch (only in E-beam evaporator Temescal) | RF Ar clean | RF Ar clean | |
| Layer thickness | 10 Å to 1 µm * | 10 Å to 1 µm * | 10 Å to 5000 Å ** | 10 Å to 5000 Å ** |
| Deposition rate | 1-10 Å/s | 1-10 Å/s | Depends on process parameters, about 1 Å/s | Depends on process parameters, at least ~ 4 Å/s, see conditions here |
| Batch size |
|
|
|
|
| Allowed materials |
|
Almost any that does not degas. See the cross-contamination sheet. |
|
|
| Comment |
|
|
* To deposit a cumulative thickness above 600 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine
** To deposit a cumulative thickness above 200 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine
Quality control of e-beam evaporated Ni films
| Quality control (QC) for Wordentec | ||||||||||||||||
|
Nickel deposition is tested occasionally, around 1-2 times per year. LabManager links require login.
Thickness is measured in 5 points with a stylus profiler. |
| Quality control (QC) for the Temescal | ||||||||||||||||||
|
Nickel deposition is tested occasionally, around 1 time per year. LabManager links require login.
Thickness is measured in 5 points with a stylus profiler. |