'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Aluminium click here]''' | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Aluminium click here]''' | ||
<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b></i> | |||
<br clear="all" /> | <br clear="all" /> | ||
| Line 13: | Line 15: | ||
*[[/Sputter rates for Al|Sputtering of Aluminium in the Wordentec]] | *[[/Sputter rates for Al|Sputtering of Aluminium in the Wordentec]] | ||
*[[/Al sputtering in Sputter System (Lesker) |Al sputtering in Sputter System (Lesker)]] | |||
*[[/Al_Sputtering_in_Cluster_Lesker_PC3 |Al Sputtering in Sputter-System Metal-Nitride(PC3)]] | |||
==E-beam evaporation of Aluminium== | ==E-beam evaporation of Aluminium== | ||
Aluminium can be deposited by e-beam assisted evaporation in the Wordentec | Aluminium can be deposited by e-beam assisted evaporation in the Wordentec and the two Temescal tools. | ||
*[[/Al Ebeam evaporation in Temescal |E-beam evaporation of Al in Temescal]] | |||
*[[/Notes on low oxygen content in e-beam prepared Al thin films|Notes on low oxygen content in e-beam prepared Al thin films (Temescal)]] | |||
<!----> | <!----> | ||
| Line 42: | Line 50: | ||
! | ! | ||
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal| | ! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]] and [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]]) | ||
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]]) | ! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]]) | ||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]]) | ! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]]) | ||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System (Lesker)]]) | ! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System (Lesker)]]) | ||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system| | ! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]]) | ||
! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]]) | ! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]]) | ||
! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/thermalevaporator|Thermal Evaporator]]) | ! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/thermalevaporator|Thermal Evaporator]]) | ||
| Line 54: | Line 61: | ||
! General description | ! General description | ||
| | | | ||
E-beam deposition of Aluminium | E-beam deposition of Aluminium | ||
| Line 73: | Line 78: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Pre-clean | ! Pre-clean | ||
|Ar ion etch | |Ar ion etch (only in E-beam evaporator Temescal) | ||
| | | | ||
| | | | ||
|RF Ar clean | |RF Ar clean | ||
|RF Ar clean | |RF Ar clean | ||
| | | | ||
| | | | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Layer thickness | ! Layer thickness | ||
|10Å to 1 µm* | |10Å to 1 µm* | ||
|10Å to 1 µm* | |10Å to 1 µm* | ||
|10Å to ~0.5µm | |10Å to ~0.5µm | ||
|10Å to ~0.5µm (very time consuming ) | |10Å to ~0.5µm (very time consuming ) | ||
|10Å to ~0.5µm | |10Å to ~0.5µm | ||
|10Å to 0. | |10Å to 0.12 µm | ||
|10Å to 1 µm | |10Å to 1 µm* | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Deposition rate | ! Deposition rate | ||
| | |1Å/s to 10Å/s | ||
| | |1Å/s to 15Å/s | ||
|Depending on [[/Sputter rates for Al|process parameters]], up to ~2.5 Å/s | |Depending on [[/Sputter rates for Al|process parameters]], up to ~2.5 Å/s | ||
|Depending on process parameters at least up to 0. | |Depending on [[/Al sputtering in Sputter System (Lesker) |process parameters]] at least up to 0.7 Å/s | ||
|Depending on process parameters at least up to 1.3 Å/s | |Depending on process parameters at least up to 1.3 Å/s. See conditions [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|here]] | ||
|~1.5 Å/s to 2 Å/s | |~1.5 Å/s to 2 Å/s | ||
|0.5, 1, or 2 Å/s | |0.5, 1, or 2 Å/s | ||
| Line 108: | Line 110: | ||
| | | | ||
*Up to 4x6" or 3x8" wafers | *Up to 4x6" or 3x8" wafers | ||
*smaller pieces | *smaller pieces | ||
| | | | ||
| Line 133: | Line 132: | ||
*6x6" wafers | *6x6" wafers | ||
| | | | ||
*Up to one 8" wafer (limited uniformity on large substrates) | *Up to 3 x 4" wafers or one 6" or 8" wafer (limited uniformity on large substrates) | ||
*Many small chips | |||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
| Line 140: | Line 140: | ||
| | | | ||
Approx. 20 min | Approx. 20 min | ||
| | | | ||
Approx. 1 hour | Approx. 1.5 hour | ||
| | | | ||
Approx. 1 hour | Approx. 1.5 hour | ||
| | | | ||
Approx. 10 min | Approx. 10 min | ||
| Line 151: | Line 149: | ||
Approx. 5 min plus 6 min transfer time | Approx. 5 min plus 6 min transfer time | ||
| | | | ||
Approx. 1 hour | Approx. 1.5 hour | ||
| | | | ||
Approx. 15 min | Approx. 15 min | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Allowed | ! Allowed materials | ||
| | | | ||
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=511 cross-contamination sheet]. | |||
| | | | ||
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=167 cross-contamination sheet]. | |||
| | | | ||
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=167 cross-contamination sheet]. | |||
| | | | ||
* Silicon wafers | * Silicon wafers | ||
* and almost any | * and almost any | ||
| | | | ||
* | *Almost that does not degas - see cross contamination sheets for [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3] | ||
* Special carrier for III-V materials. | |||
| | | | ||
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=167 cross-contamination sheet]. | |||
| | | | ||
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=404 cross-contamination sheet]. | |||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Comment | ! Comment | ||
|'''*''' Thickness above 600 nm: ask for permission | |'''*''' Thickness above 600 nm: ask for permission | ||
It is possible to tilt the substrate. | It is possible to tilt the substrate. | ||
|'''*''' Thickness above 600 nm: ask for permission. | |'''*''' Thickness above 600 nm: ask for permission. | ||
| Line 268: | Line 189: | ||
| | | | ||
| | | | ||
|''' | |'''**'''Thickness above 120 nm: ask for permission | ||
| | | | ||
|} | |} | ||
'''*''' ''For | '''*''' ''For cumulative deposition above 600 nm please write to metal@nanolab.dtu.dk to make sure there will be enough Al for your deposition'' | ||
==Aluminium deposition on ZEP520A for lift-off - comparison of thermal and e-beam evaporation == | ==Aluminium deposition on ZEP520A for lift-off - comparison of thermal and e-beam evaporation == | ||