Jump to content

Specific Process Knowledge/Thermal Process/Pyrolysis/Pyrolysis with Multipurpose Anneal Furnace: Difference between revisions

From LabAdviser
Longq (talk | contribs)
No edit summary
Pevo (talk | contribs)
No edit summary
 
(25 intermediate revisions by one other user not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thermal_Process/Pyrolysis/Pyrolysis_with_Multipurpose_Anneal_Furnace click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thermal_Process/Pyrolysis/Pyrolysis_with_Multipurpose_Anneal_Furnace click here]'''  
''This page is written by DTU Nanolab internal''


==Pyrolysis Recipes==
==Pyrolysis Recipes==


Because the properties of the final carbon are largely depending on the pyrolysis process as well as the polymer precusors, each parameter has a different influence. By modifying those parameters, the properties of pyrolytic carbon can be tailored. The number of steps, the maximum temperature of each step, the heating rate, the dwell time at the maximum temperature and the gas composition inside the furnace are the parameters that can be changed to control the properties of pyrolytic carbon. At DTU Nanolab, the polymer precusor mostly is SU-8 negative photoresist and high temperature 3D printing resin. Depend on the designed properties of pyrolytic carbon material, pyrolysis process will be optimized. Check the recipes on the Pyrolysis with Multipurpose Anneal Furnace page below.
Because the properties of the final carbon are largely depending on the pyrolysis process as well as the polymer precusors, each parameter has a different influence. By modifying those parameters, the properties of pyrolytic carbon can be tailored. The number of steps, the maximum temperature of each step, the heating rate, the dwell time at the maximum temperature and the gas composition inside the furnace are the parameters that can be changed to control the properties of pyrolytic carbon. At DTU Nanolab, the polymer precusor mostly is SU-8 negative photoresist and high temperature 3D printing resin. Depend on the designed properties of pyrolytic carbon material, pyrolysis process will be optimized.
 
=== Optimized Recipe for the conductivity of pyrolytic carbon ===
 
For using pyrolytic carbon as a working electrode for electrochemical sensor, the conductivity of the pyrolytic carbon must be maximized. The main goal of this recipe is to obtain the carbon material with highest conductivity as possible. The conductivity is measured by probe station with 4 points probe method.
 
Recipe: ""
 
[[File:1_step_pyrolysis.png|400px|]]
 
{| class="wikitable"
|-
! Parameter
! Value
|-
| Precusor
| SU-8
|-
| Number of step
| 1
|-
| Final Temperature
| 1100<sup>o</sup>C
|-
| Ramping Rate
| 2<sup>o</sup>C per minute
|-
| Annealing time at final temperature
| 6 hours
|-
| Gas
| 20 sccm N<sub>2</sub>
|}
 
=== Optimized Recipe for the stress of pyrolytic carbon ===
 
Recipe for maximize the tensile stress of pyrolytic carbon material. The stress is measured by the DektakXTA by thin film stress method.
 
Recipe: "Long_optimized"
 
[[File:2_step_pyrolysis.png|400px|]]
 
{| class="wikitable"
|-
! Parameter
! Value
|-
| Precusor
| SU-8
|-
| Number of step
| 2
|-
| First step Temperature
| 200<sup>o</sup>C
|-
| First step Anneal time
| 30 minutes
|-
| First step Ramping Rate
| 2<sup>o</sup>C per minute
|-
| Final temperature
| 700<sup>o</sup>C
|-
| Ramping rate to final temperature
| 30<sup>o</sup>C per minute
|-
| Annealing time at final temperature
| 10 minutes
|-
| Gas
| 20 sccm N<sub>2</sub>
|}
 
=== Optimized Recipe for the porous structure of pyrolytic carbon ===
 
This recipe is applied for High temperature 3D printing resin in order to obtain the high porous structure of pyrolytic carbon material. The structure is characterized by SEM image.
 
Recipe: ""
 
[[File:3_step_pyrolysis.png|400px|]]


== Recipe for maximize the tensile stress of pyrolytic carbon ==
{| class="wikitable"
|-
! Parameter
! Value
|-
| Precusor
| High temperature 3D printing resin
|-
| Number of step
| 3
|-
| First step Temperature
| 375<sup>o</sup>C
|-
| First step Anneal time
| 3 hours
|-
| First step Ramping Rate
| 2<sup>o</sup>C per minute
|-
| Second step Temperature
| 425<sup>o</sup>C
|-
| Second step Anneal time
| 30 minutes
|-
| Second step Ramping Rate
| 1<sup>o</sup>C per minute
|-
| Final temperature
| 900<sup>o</sup>C
|-
| Ramping rate to final temperature
| 2<sup>o</sup>C per minute
|-
| Annealing time at final temperature
| 1 hour
|-
| Gas
| 20 sccm N<sub>2</sub>
|}

Latest revision as of 10:30, 19 June 2023

Feedback to this page: click here

This page is written by DTU Nanolab internal


Pyrolysis Recipes

Because the properties of the final carbon are largely depending on the pyrolysis process as well as the polymer precusors, each parameter has a different influence. By modifying those parameters, the properties of pyrolytic carbon can be tailored. The number of steps, the maximum temperature of each step, the heating rate, the dwell time at the maximum temperature and the gas composition inside the furnace are the parameters that can be changed to control the properties of pyrolytic carbon. At DTU Nanolab, the polymer precusor mostly is SU-8 negative photoresist and high temperature 3D printing resin. Depend on the designed properties of pyrolytic carbon material, pyrolysis process will be optimized.

Optimized Recipe for the conductivity of pyrolytic carbon

For using pyrolytic carbon as a working electrode for electrochemical sensor, the conductivity of the pyrolytic carbon must be maximized. The main goal of this recipe is to obtain the carbon material with highest conductivity as possible. The conductivity is measured by probe station with 4 points probe method.

Recipe: ""

Parameter Value
Precusor SU-8
Number of step 1
Final Temperature 1100oC
Ramping Rate 2oC per minute
Annealing time at final temperature 6 hours
Gas 20 sccm N2

Optimized Recipe for the stress of pyrolytic carbon

Recipe for maximize the tensile stress of pyrolytic carbon material. The stress is measured by the DektakXTA by thin film stress method.

Recipe: "Long_optimized"

Parameter Value
Precusor SU-8
Number of step 2
First step Temperature 200oC
First step Anneal time 30 minutes
First step Ramping Rate 2oC per minute
Final temperature 700oC
Ramping rate to final temperature 30oC per minute
Annealing time at final temperature 10 minutes
Gas 20 sccm N2

Optimized Recipe for the porous structure of pyrolytic carbon

This recipe is applied for High temperature 3D printing resin in order to obtain the high porous structure of pyrolytic carbon material. The structure is characterized by SEM image.

Recipe: ""

Parameter Value
Precusor High temperature 3D printing resin
Number of step 3
First step Temperature 375oC
First step Anneal time 3 hours
First step Ramping Rate 2oC per minute
Second step Temperature 425oC
Second step Anneal time 30 minutes
Second step Ramping Rate 1oC per minute
Final temperature 900oC
Ramping rate to final temperature 2oC per minute
Annealing time at final temperature 1 hour
Gas 20 sccm N2