Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-2/Black silicon on Demand: Difference between revisions

Vthongu (talk | contribs)
No edit summary
Jmli (talk | contribs)
No edit summary
(37 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page:  
'''Feedback to this page:  
[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-2/Black silicon on Demand click here]'''
[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-2/Black silicon on Demand click here]'''
<!-- Page reviewed 9/8-2022 jmli -->
 
{{cc-vthongu1}}


Black silicon (BSi or silicon micro/nano-grass) is a frequently encountered phenomenon in highly directional etching of silicon using mainstream plasma etch tools. Because of the almost perfect light absorption, BSi has found a prominent place in photovoltaic applications. The strongly increased surface area has also shown attractive opportunities in chemical and optical devices. In addition, another already established characteristic of BSi is its ability to prevent cell growth and as such creates anti-bacterial, anti-fogging and self-cleaning surfaces.  
Black silicon (BSi or silicon micro/nano-grass) is a frequently encountered phenomenon in highly directional etching of silicon using mainstream plasma etch tools. Because of the almost perfect light absorption, BSi has found a prominent place in photovoltaic applications. The strongly increased surface area has also shown attractive opportunities in chemical and optical devices. In addition, another already established characteristic of BSi is its ability to prevent cell growth and as such creates anti-bacterial, anti-fogging and self-cleaning surfaces.  
Line 8: Line 11:
On DRIE-Pegasus 2, the formation and controllabilty of BSi in the CORE sequence is different from how BSi presents itself in the FC-based sequences. The schematic illustration of BSi formation in the Bosch process and BSi-free in the CORE sequence is shown below.
On DRIE-Pegasus 2, the formation and controllabilty of BSi in the CORE sequence is different from how BSi presents itself in the FC-based sequences. The schematic illustration of BSi formation in the Bosch process and BSi-free in the CORE sequence is shown below.


[[File:Figure_2.png|400px|center|thumb]]
[[File:Figure_2.png|400px]]


Example of the CORE recipe for BSi  
Example of the CORE recipe for BSi  
Line 16: Line 19:
Silicon wafers are prepared with 1.5 μm thick resist patterns (AZ MIR 701 DUV resist from MicroChemicals) and exposed using a maskless aligner (MLA150, Heidelberg) to create patterns above 400 nm. Below are some SEM images of BSi nanostructures achieved by the modified CORE process:
Silicon wafers are prepared with 1.5 μm thick resist patterns (AZ MIR 701 DUV resist from MicroChemicals) and exposed using a maskless aligner (MLA150, Heidelberg) to create patterns above 400 nm. Below are some SEM images of BSi nanostructures achieved by the modified CORE process:


[[File:BSi free.png|400px|left|thumb|''''' 1 µm silicon pillars etched with a BSi-free recipe''''']]
<gallery caption="" widths="360px" heights="280px" perrow="2">
 
File:BSi free.png|''''' 1 µm silicon pillars etched with a BSi-free recipe'''''
[[File:BSi full.png|400px|left|thumb|''''' 1 µm silicon pillars etched first with a BSi-free recipe and then continued with a BSi-full recipe''''']]
File:BSi full.png|''''' 1 µm silicon pillars etched first with a BSi-free recipe and then continued with a BSi-full recipe'''''
</gallery>


[[File:PR strip.png|800px|left|thumb|''''' By removing the mask on top of the pillars, the BSi can be formed on top of the these pillars''''']]
[[File:PR strip.png|800px|left|thumb|''''' By removing the mask on top of the pillars, the BSi can be formed on top of the these pillars''''']]


<br clear="all" />
For more details, please contact Henri Jansen (henrija@dtu.dk) or Vy Thi Hoang Nguyen (vthongu@dtu.dk).
For more details, please contact Henri Jansen (henrija@dtu.dk) or Vy Thi Hoang Nguyen (vthongu@dtu.dk).