Jump to content

Specific Process Knowledge/Thermal Process/Oxidation/Standard oxidation recipes: Difference between revisions

From LabAdviser
Pevo (talk | contribs)
Paphol (talk | contribs)
No edit summary
(14 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thermal_Process/Oxidation/Standard_oxidation_recipes click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thermal_Process/Oxidation/Standard_oxidation_recipes click here]'''


''This page is written by DTU Nanolab  internal''
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>=
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>=


Line 6: Line 7:
The oxidation furnaces in the cleanroom are being used for dry and wet oxidation of silicon wafers.  
The oxidation furnaces in the cleanroom are being used for dry and wet oxidation of silicon wafers.  


On this page the steps in the standard oxidation recipes on the furnaces will be listet.  
On this page the steps in the standard oxidation recipes on the furnaces will be listed.  
   
   


Line 32: Line 33:


The wet oxidation recipes in the A-stack, C1 and C3 furnaces are very similar.  
The wet oxidation recipes in the A-stack, C1 and C3 furnaces are very similar.  
However, there are a few differences in recipes, because water vapour can be generated by either a torch, a steamer or a bubbler. More information can be found on each furnace page.


Wet oxidation of III-V sample in the C2 furnace is described here:
Wet oxidation of III-V sample in the C2 furnace is described here:


http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thermal_Process/Oxidation/Oxidation_on_III-V_oxidation_furnace_(C2)
http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thermal_Process/Oxidation/Oxidation_on_III-V_oxidation_furnace_(C2)


===General recipe remarks:===
===General recipe remarks:===
Line 57: Line 59:
==Dry oxidation recipe steps==
==Dry oxidation recipe steps==


0 STANDBY
'''00 STANDBY'''
Message: "Standby"


The furnace is
''Message: "Standby"''


This will be the active step, when the furnace is not in use, and when a recipe is selected.


If a recipe is aborted, it will also jump to the STANDBY step.


In the standby step, the furnace is closed and kept clean by an N<sub>2</sub> flow.


Temperature: 700 C
*Standby temperature: 700 <sup>o</sup>C
N2 flow: 3 SLM
*N<sub>2</sub> flow: 3 SLM
Furnace closed
*O<sub>2</sub> flow: 0 SLM


The user has to press "Start" (on the touch screen or furnace computer) to start the recipe.
The user has to press "Start" (on the touch screen or furnace computer) to start the recipe.


It a dry oxidation recipe is aborted, it will jump to the "Standby" step.


*LM-LOCK
'''01 LM-LOCK'''
Message: "Standby"
 
The recipe can only continue, if a user is logged on in LabManager
The recipe can only continue, if a user is logged on in LabManager, otherwise the furnace will shown an alarm (digital input 6) after 1 minute.
 
 
'''02 OPEN'''
 
''Message: "Boat moving"''


*OPEN
Message: "Boat moving"
The furnace opens
The furnace opens


*LOAD WAFERS
Message: "Load wafers
Wafers are loaded in furnace.


The user has to press "Start" (on the touch screen) or "Continue" (on the furnace computer) to close the furnace   
'''03 LOAD WAFERS'''
 
''Message: "Load wafers''
 
When the furnace is open, the user can load wafers in the furnace.
 
The quartz boat for the wafers is located in furnace, so it has to be liftet down on the quartz plate, before the wafers are loaded.
 
After the wafers are loaded, the user has to press "Start" (on the touch screen) or "Continue" (on the furnace computer) to close the furnace.    


*CLOSE
Message: "Boat moving"
The furnace is closing


*HEAT UP
'''04 CLOSE'''
Message: "Heat-up"
The furnace is heating up to the temperature defined in the recipe
The recipe will continue to the next step, when the temperature of center heating zone (zone 2) reached the right temperature


*OXIDATION
''Message: "Boat moving"''
Message: "Dry oxidation"


The dry oxidation is started
The furnace closes.
O2 flow: 5 SLM
N2 flow: 0 SLM


The oxidation time is a variable command.


has been defined by the user. The oxidation time can be changed, until the oxidation step is started.
'''05 HEAT UP'''


*ANNEAL
''Message: "Heat-up"''
Message: "Anneals/Dens"


*COOL DOWN
The furnace heats up to the temperature defined in the recipe (usually 800-1150 <sup>o</sup>C).
Message: "Cool-down"


The furnace is cooling down to 700 C (the standby temperature)
The recipe will continue to the next step, when the temperature of center heating zone (zone 2) reaches the right temperature.


*UNLOAD WAFERS
Message: "Unload wafers"


The user has to press "Start" (on the touch screen) or "Continue" (on the furnace computer) to close the furnace 
'''06 OXIDATION'''


*OPEN
''Message: "Oxidation"''
Message: "Open"


The furnace opens.
The dry oxidation is started by flowing O<sub>2</sub> through the furnace instead of N<sub>2</sub.
 
*O<sub>2</sub> flow: 5 SLM
*N<sub>2</sub> flow: 0 SLM
 
The oxidation time is a variable command, so it can be set by the user. 
 
The oxidation time can be changed, until the oxidation step is started.
 
 
'''07 ANNEAL'''
 
''Message: "Anneal/Dens"''
 
The O<sub>2</sub> gas is purged out of the furnace by an N<sub>2</sub> flow, so that the oxidation stop.
 
The wafers are annealed in N<sub>2</sub> at the same temperature as the oxidation temperature. The annealing will improve the oxide quality by making it more dense.
 
*N<sub>2</sub> flow: 6 SLM
*O<sub>2</sub> flow: 0 SLM
 
Normally the annealing time is 20 minutes, but it is a variable command, so it can be set by the user. 
 
The annealing time can be changed, until the annealing step is started.
 
 
'''08 COOL DOWN'''
 
''Message: "Cool-down"''
 
The furnace is cooling down to 700 <sup>o</sup>C (the standby temperature)
 
 
'''09 UNLOAD WAFERS'''
 
''Message: "Unload wafers"''
 
The recipe is paused, until the user presses "Start" (on the touch screen) or "Continue" (on the furnace computer). 
 
 
'''10 OPEN'''


*UNLOAD
''Message: "Open"''
Message: "Unload wafers"


When the furnace is open, the wafer can be unloaded.
The furnace opens.
Be aware of, that the wafers are very hot, so they have to cool down for about five minutes


When the wafers are unloaded, the user has to press "Start" (on the touch screen) or "Continue" (on the furnace computer) to close the furnace.
The recipe then jumps to the STANDBY step, and the user can leave the furnace, after it has closed. 


If a recipe is aborted
'''11 UNLOAD'''


''Message: "Unload wafers"''


When the furnace is open, the wafers can be unloaded.


Place the boat on the quartz plate in front of the furnace to unload the wafers. And be aware of, that the wafers are very hot, so they have to cool down for a few minutes, before they are removed from the boat.


The standard annealing time is 20 minutes, but users can change the time. The annealing time can be changed, until the annealing step is started.
When the wafers are unloaded, the user has to press "Start" (on the touch screen) or "Continue" (on the furnace computer) to close the furnace.
The recipe then jumps to the STANDBY step, and the user can leave the furnace, after it has closed.

Revision as of 10:49, 7 February 2023

Feedback to this page: click here

This page is written by DTU Nanolab internal

THIS PAGE IS UNDER CONSTRUCTION

The oxidation furnaces in the cleanroom are being used for dry and wet oxidation of silicon wafers.

On this page the steps in the standard oxidation recipes on the furnaces will be listed.


Dry oxidation can be done in the these furnaces:

  • A1 Boron Drive-in and Pre-dep furnace
  • A2 Gate Oxide furnace
  • A3 Phosphorus Pre-dep furnace
  • C1 Anneal-Oxide furnace
  • C3 Anneal-Bond furnace
  • Multipurpose Anneal furnace

The dry oxidation recipes in the A- and C-stack furnaces are very similar and will be described on this page.

There are no standard recipes on the Multipurpose Anneal furnace, so no oxidation recipes will be described here.


Wet oxidation can be done in these furnaces:

  • A1 Boron Drive-in and Pre-dep furnace
  • A3 Phosphorus Pre-dep furnace
  • C1 Anneal-Oxide furnace
  • C2 III-V Oxidation furnace
  • C3 Anneal-Bond furnace

The wet oxidation recipes in the A-stack, C1 and C3 furnaces are very similar.

However, there are a few differences in recipes, because water vapour can be generated by either a torch, a steamer or a bubbler. More information can be found on each furnace page.

Wet oxidation of III-V sample in the C2 furnace is described here:

http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thermal_Process/Oxidation/Oxidation_on_III-V_oxidation_furnace_(C2)

General recipe remarks:

The oxidation temperature is fixed in each recipe. The temperature can be seen in the recipe name, e.g. "DRY1000" for dry oxidation at 1000 C and "WET1100" for wet oxidation at 1100 C.

The oxidation and annealing times are variable commands in oxidation recipe. It means that these can be changed by the users.

The oxid thickness is defined by the oxidation time. Wet oxidation is much faster then dry oxidation. It is maximum allowed to grow 300 nm of dry oxide and 3 um of wet oxidation.

The annealing improves... The standard annealing time is 20 minutes, but it is possible to change the time.





Dry oxidation recipe steps

00 STANDBY

Message: "Standby"

This will be the active step, when the furnace is not in use, and when a recipe is selected.

If a recipe is aborted, it will also jump to the STANDBY step.

In the standby step, the furnace is closed and kept clean by an N2 flow.

  • Standby temperature: 700 oC
  • N2 flow: 3 SLM
  • O2 flow: 0 SLM

The user has to press "Start" (on the touch screen or furnace computer) to start the recipe.


01 LM-LOCK

The recipe can only continue, if a user is logged on in LabManager, otherwise the furnace will shown an alarm (digital input 6) after 1 minute.


02 OPEN

Message: "Boat moving"

The furnace opens


03 LOAD WAFERS

Message: "Load wafers

When the furnace is open, the user can load wafers in the furnace.

The quartz boat for the wafers is located in furnace, so it has to be liftet down on the quartz plate, before the wafers are loaded.

After the wafers are loaded, the user has to press "Start" (on the touch screen) or "Continue" (on the furnace computer) to close the furnace.


04 CLOSE

Message: "Boat moving"

The furnace closes.


05 HEAT UP

Message: "Heat-up"

The furnace heats up to the temperature defined in the recipe (usually 800-1150 oC).

The recipe will continue to the next step, when the temperature of center heating zone (zone 2) reaches the right temperature.


06 OXIDATION

Message: "Oxidation"

The dry oxidation is started by flowing O2 through the furnace instead of N2</sub.

  • O2 flow: 5 SLM
  • N2 flow: 0 SLM

The oxidation time is a variable command, so it can be set by the user.

The oxidation time can be changed, until the oxidation step is started.


07 ANNEAL

Message: "Anneal/Dens"

The O2 gas is purged out of the furnace by an N2 flow, so that the oxidation stop.

The wafers are annealed in N2 at the same temperature as the oxidation temperature. The annealing will improve the oxide quality by making it more dense.

  • N2 flow: 6 SLM
  • O2 flow: 0 SLM

Normally the annealing time is 20 minutes, but it is a variable command, so it can be set by the user.

The annealing time can be changed, until the annealing step is started.


08 COOL DOWN

Message: "Cool-down"

The furnace is cooling down to 700 oC (the standby temperature)


09 UNLOAD WAFERS

Message: "Unload wafers"

The recipe is paused, until the user presses "Start" (on the touch screen) or "Continue" (on the furnace computer).


10 OPEN

Message: "Open"

The furnace opens.


11 UNLOAD

Message: "Unload wafers"

When the furnace is open, the wafers can be unloaded.

Place the boat on the quartz plate in front of the furnace to unload the wafers. And be aware of, that the wafers are very hot, so they have to cool down for a few minutes, before they are removed from the boat.