Jump to content

Specific Process Knowledge/Etch/ICP Metal Etcher/Titanium: Difference between revisions

From LabAdviser
Jml (talk | contribs)
Created page with "=== Titanium etch === {| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" |+ '''Ti etch''' |- ! Parameter ! width="200" | Process 1 ! width="200" | Proc..."
 
Jmli (talk | contribs)
No edit summary
(7 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/Titanium click here]'''
<!--Checked for updates on 5/10-2020 - ok/jmli -->
<!--Checked for updates on 30/7-2018 - ok/jmli -->
=== Titanium etch ===
=== Titanium etch ===
{{Template:Author-jmli1}}
<!--Checked for updates on 2/02-2023 - ok/jmli -->





Revision as of 15:05, 2 February 2023

Feedback to this page: click here

Titanium etch

Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab


Ti etch
Parameter Process 1 Process 2
Cl2 (sccm) 30 30
HBr (sccm) - -
Pressure (mTorr) 3, Strike 3 secs @ 15 mTorr??? 3
Coil power (W) 800 900
Platen power (W) 100 50
Temperature (oC) 20 20
Spacers (mm) 30 30
Etch rate (nm/min) 152 64
AZ resist selectivity 0.67 0.83