Specific Process Knowledge/Thermal Process/A4 Phosphor Pre-dep furnace: Difference between revisions

From LabAdviser
No edit summary
Paphol (talk | contribs)
 
(16 intermediate revisions by 4 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thermal_Process/A4_Phosphor_Pre-dep_furnace click here]'''
'''Feedback to this page''': '''[mailto:thinfilm@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thermal_Process/A4_Phosphor_Pre-dep_furnace click here]'''


==Phosphorus Predep furnace (A4)==
''This page is written by DTU Nanolab  internal''
[[Image:A4.JPG|thumb|300x300px|A4 Phosphor Pre-dep furnace. Positioned in cleanroom 2]]
[[Category: Equipment |Thermal A4]]
[[Category: Thermal process|Furnace]]
[[Category: Furnaces|A4]]


The Phosphorus Predep furnace (A4) is used to dope Si wafers with phosphorus to make conductive structures, etch stop layers etc. The doping source is phosphoryl chloride (commonly called phosphorus oxychloride) which is a colourless liquid with the formula POCl<sub>3</sub>.
==Phosphorus Pre-dep furnace (A4)==
[[Image:A4.JPG|thumb|300x300px|Phosphorus Pre-dep furnace (A4). Positioned in cleanroom B-1/ Photo: DTU Nanolab internal]]
 
The Phosphorus Pre-dep furnace (A4) is used to dope Si wafers with phosphorus to make conductive structures, etch stop layers etc. The doping source is phosphoryl chloride (commonly called phosphorus oxychloride) which is a colourless liquid with the chemical formula POCl<sub>3</sub>.
 
A4 is the lowest furnace tube in the A-stack positioned in cleanroom B-1. The furnaces in the A-stack are the cleanest of all furnaces in the cleanroom. Be aware of that all wafers (including new wafers) have to be RCA cleaned before they enter the furnace, and please check the cross contamination information in LabManager before you use the furnace.  


A4 is the lowest furnace tube in the A-stack positioned in cleanroom 2. The A-stack together with the Gate Oxide furnace (C2) are the cleanest of all furnaces in the cleanroom. Please be aware of which substrates are allowed to enter this furnace. Check the [http://www.labmanager.danchip.dtu.dk/view_binary.php?fileId=1250 cross contamination chart].


'''The user manual, technical information and contact information can be found in LabManager:'''
'''The user manual, technical information and contact information can be found in LabManager:'''


'''[http://www.labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=47 Phosphorus Predep furnace (A4)]'''
'''[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=83 Phosphorus Pre-dep furnace (A4)]'''


== Process knowledge ==
== Process knowledge ==
*[[Specific Process Knowledge/Thermal Process/Dope with Phosphorus|Dope with Phosphorus]]
*[[Specific Process Knowledge/Thermal Process/Dope with Phosphorus|Dope with Phosphorus]]


==Overview of the performance of the Phosphor pre-dep furnace and some process related parameters==
==Overview of the performance of the Phosphorus Pre-dep furnace and some process related parameters==


{| border="2" cellspacing="0" cellpadding="0"  
{| border="2" cellspacing="0" cellpadding="2"  
|-
|-
!style="background:silver; color:black;" align="center"|Purpose  
!style="background:silver; color:black;" align="center"|Purpose  
|style="background:LightGrey; color:black"|Doping of Phosphor
|style="background:WhiteSmoke; color:black"|
|-
!style="background:silver; color:black" align="center"|Performance
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Look at Process knowladge
*Phosphorus doping/pre-deposition using POCl<sub>3</sub>
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameter range
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameter range
Line 36: Line 37:
|style="background:LightGrey; color:black"|Process pressure
|style="background:LightGrey; color:black"|Process pressure
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*1 atm
*1 atm (atmospheric pressure)
|-
|-
|style="background:LightGrey; color:black"|Gasses on the system
|style="background:LightGrey; color:black"|Gasses on the system
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|


*POCl<sub>3</sub>, N<sub>2</sub>
*POCl<sub>3</sub>
*N<sub>2</sub>
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Substrates
|style="background:LightGrey; color:black"|Batch size
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*1-30 4" wafer (or 2" wafers) per run
*1-30 100 mm wafers  
|-
|-
| style="background:LightGrey; color:black"|Substrate material allowed
| style="background:LightGrey; color:black"|Substrate materials allowed
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Silicon wafers (new from the box or RCA cleaned)
*Silicon wafers (RCA cleaned)
*In doubt: look at the [http://www.labmanager.danchip.dtu.dk/view_binary.php?fileId=1250 cross contamination chart] or please send a mail to [mailto:furnace@danchip.dtu.dk furnace@danchip.dtu.dk]
|-
|-
|}
|}

Latest revision as of 15:08, 31 January 2023

Feedback to this page: click here

This page is written by DTU Nanolab internal

Phosphorus Pre-dep furnace (A4)

Phosphorus Pre-dep furnace (A4). Positioned in cleanroom B-1/ Photo: DTU Nanolab internal

The Phosphorus Pre-dep furnace (A4) is used to dope Si wafers with phosphorus to make conductive structures, etch stop layers etc. The doping source is phosphoryl chloride (commonly called phosphorus oxychloride) which is a colourless liquid with the chemical formula POCl3.

A4 is the lowest furnace tube in the A-stack positioned in cleanroom B-1. The furnaces in the A-stack are the cleanest of all furnaces in the cleanroom. Be aware of that all wafers (including new wafers) have to be RCA cleaned before they enter the furnace, and please check the cross contamination information in LabManager before you use the furnace.


The user manual, technical information and contact information can be found in LabManager:

Phosphorus Pre-dep furnace (A4)

Process knowledge

Overview of the performance of the Phosphorus Pre-dep furnace and some process related parameters

Purpose
  • Phosphorus doping/pre-deposition using POCl3
Process parameter range Process Temperature
  • 900-1150 oC
Process pressure
  • 1 atm (atmospheric pressure)
Gasses on the system
  • POCl3
  • N2
Substrates Batch size
  • 1-30 100 mm wafers
Substrate materials allowed
  • Silicon wafers (RCA cleaned)