GaAs/AlGaAs etching using III-V ICP

Recipes developed and/or tested by DTU Photonics internal before 2011

Recipe GaAs Etch
Cl2 flow 4 sccm
Ar flow 12 sccm
Platen power 80 W
Coil power 700 W
Pressure 6 mTorr
Platen chiller temperature 20oC


Results (GaAs Etch)
GaAs etch rate >500 nm/min
Sidewall angle ~ 85-90o
Selectivity (GaAs:Si3N4, GaAs:AlInP) 10:1, 5:1


Recipe GaAs_AlGaAs Etch
Cl2 flow 20 sccm
N2 flow 50 sccm
Platen power 100 W
Coil power 600 W
Pressure 2 mTorr
Platen chiller temperature 20oC


Results (GaAs_AlGaAs Etch)
AlGaAs etch rate >1000 nm/min
Sidewall angle ~ 90o
Selectivity (GaAs:SiO2) 30:1


Recipe GaAs_AlGaAs Etch_BCl3
Cl2 flow 10 sccm
BCl3 flow 10 sccm
Ar flow 10 sccm
N2 flow 4 sccm
Platen power 50 W
Coil power 500 W
Pressure 1 mTorr
Platen chiller temperature 20oC


Results (GaAs_AlGaAs Etch_BCl3)
GaAs etch rate >750 nm/min
Sidewall angle 85-90o
Selectivity (GaAs:Si3N4, GaAs:AlInP) 10:1
 
Result of GaAs etching with BCl3. Done by: Qijiang Ran, DTU Photonics, 2011.