AR-N 7520 New is a negative resist provided by Allresist. The "New" is important, "AR-N 7520" and "AR-N 7520 New" are not the same resists.

Contrast curve

  • Coater: LabSpin 2
  • Substrate: 2" Si
  • Acceleration: 1000 RPM/s
  • Speed: 4000 RPM
  • Time: 60 s
  • Baking temperature: 85C
  • Baking time: 60 s
  • Exposure: 100 kV (JEOL 9500)
  • Development: AR 300-46 for 90 seconds
  • Stopper: DI for 30 seconds + blow dry with nitrogen


 

AR-N 7520.17 New contrast curve.