Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/Slow etch

From LabAdviser

The slow etch

The slow etch is designed to etch slow at low powers to etch thin films and to avoid overheating of samples mounted on a carrier with Capton/polyimide tape

Parameter Recipe name: Slow Etch
Coil Power [W] 350
Platen Power [W] 50
Platen temperature [oC] 20
He flow [sccm] 0
CF4 flow [sccm] 40
Pressure [mTorr] 4
Typical results Test Results
Etch of Si3N4 with DUV mask
Etch rate of Si3N4 ~nm/min
Etch rate of Silicon ~nm/min
Etch rate of DUV resist] ~nm/min


Profile [o]