Jump to content

Specific Process Knowledge/Lithography/4562

From LabAdviser

Feedback to this section: click here

AZ 4562 is a positive UV photoresist for thick coatings (5µm and above).

Priming

Spin coating

 
Spin curves for AZ MiR 701 (29cps) using a 30s spin-off, and a 60s@90°C softbake (proximity bake for Gamma)


Exposure

Development

The recommended development speed for AZ 4562 is 2µm/min. A 6.2µm resist film thus requires 3min development, usually as three 60s puddles of TMAH (AZ 726 MIF). 10µm AZ 4562 has successfully been developed using 4x60s development