Wet Silicon Nitride Etch
|
BHF
|
RIE (Reactive Ion Etch)
|
AOE (Advanced Oxide Etch)
|
IBE/IBSD Ionfab 300
|
ICP Metal
|
| Generel description
|
- Isotropic etch
- Well suited for removing all nitride on a wafer surface (nitride strip) without a mask. High selectivity Si3N4/Si (>100) and Si3N4/SiO2 (>20) @ 160 C.
|
- Isotropic etch
- Well suited for removing all PECVD nitride on a wafer surface (nitride strip) without a mask. Etches LPCVD nitride very slowly
|
- Anisotropic etch: vertical sidewalls
|
- Anisotropic etch: vertical sidewalls
- Deep etch
|
- Primarily for pure physical etch by sputtering with Ar-ions
|
- Anisotropic etch: vertical sidewalls
|
| Possible masking materials
|
- Silicon Oxide
- PolySilicon
|
- Photoresist
- PolySilicon
- Blue film
|
- Photoresist
- DUV resist
- E-beam resist
- Silicon Oxide
- Silicon Nitride
- Aluminium
- Metals if they cover less than 5% of the wafer area (ONLY RIE2!)
|
- Photoresist
- DUV resist
- E-beam resist
- Silicon Oxide
- Silicon Nitride
- Aluminium
- Chromium (please try to avoid it)
|
- Any material that is accepted in the machine
|
- Resists
- other materials from the allowed list of materials
|
| Etch rate range
|
- Si3N4 @ 160 oC: ~26 Å/min
|
- PECVD nitride: ~400-1000 Å/min
|
- Typically 40-50 nm/min can be increased or decreased by using other recipe parameters.
|
- Process dependent.
- Tested once to ~60nm/min
|
- Process dependent.
- Has not been tested yet.
|
- Process dependent
- 60-65 nm/min has been tested
|
| Substrate size
|
|
|
- As many small samples as can be fitted on the 100mm carrier.
- #1 100mm wafer (or smaller with carrier)
- #1 150mm wafer (only when the system is set up for 150mm)
|
- As many small samples as can be fitted on a 100mm wafer
- #1 50 mm wafer fitted on a 100mm wafer
- #1 100 mm wafer
- #1 150 mm wafers (only RIE2 when set up to 150mm)
|
- As many samples as can be securely fitted on a up to 200mm wafer
- #1 50 mm wafer with special carrier
- #1 100 mm wafer with special carrier
- #1 150 mm wafers with special carrier
- #1 200 mm wafer
|
- Set up for 150mm wafers
- Smaller samples can be processes when fixed to a 150mm carrier wafer.
|
| Allowed materials
|
- Silicon
- Silicon Oxide
- Silicon Nitride
- Silicon Oxynitride
|
- Silicon
- Silicon Oxide
- Silicon Nitride
- Silicon Oxynitride
- Photoresist
- Blue film
|
- Silicon
- Silicon Oxide
- Silicon Nitride
- Silicon Oxynitride
- Photoresist
- E-beam resists
- DUV resists
- Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)
- Quartz/fused silica
|
- Silicon
- Silicon Oxide
- Silicon Nitride
- Silicon Oxynitride
- Photoresist
- E-beam resists
- DUV resists
- Aluminium
- Chromium (try to avoid it)
- Quartz/fused silica
|
- Silicon
- Silicon oxides
- Silicon (oxy)nitrides
- Metals from the +list
- Metals from the -list
- Alloys from the above list
- Stainless steel
- Glass
- III-V materials
- Resists
- Polymers
- Capton tape
|
- Silicon
- Silicon Oxide
- Silicon Nitride
- Silicon Oxynitride
- Photoresist
- E-beam resists
- DUV resists
- Aluminium (Al, Al2O3, AlN)
- Chromium
- Titanium (Ti, TiW, TiN, TiO2)
- Tungsten (W)
- Molybdynem
- Quartz/fused silica
|