Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange

From LabAdviser
Comparison of processes before and after the change of showerhead in December 2014
Process Before After
Name/Type Description Wafer ID Comment SEM images Wafer ID Comment SEM images
Continuous black silicon recipe on blank wafer 15 mins, -10 degrees, 32 mtorr, 60 sccm SF6, 55 sccm O2, 70 W platen S004592 Wafer centre S004679 Wafer centre
S004592 Wafer edge S004679 Wafer edge
Switched polysilicon etch on DUV wafer, (D/E) indicate Dep and Etch 50 cycles, 30 degrees, 2.3/5 secs, 10/10 mtorr, 0/60 sccm SF6, 0/5 sccm O2, 50/20 sccm C4F8, 600/400 W coil, 0/40 W platen S004592 Wafer centre S004679 Wafer centre
S004592 Wafer edge S004679 Wafer edge