Jump to content

Specific Process Knowledge/Etch/Etching of Aluminium

From LabAdviser

Etching of Aluminium

Etching of aluminium is done wet at Danchip. We have two different solutions:

  1. H2O:H3PO4 1:2 at 50 oC
  2. Pre-mixed etch solution: PES 77-19-04 at 20 oC
Aluminium Etch 1 Aluminium Etch 2
General description
  • Etch of pure aluminium
  • Etch of aluminium + 1.5% Si
Possible masking materials:
  • Photoresist
  • Silicon nitride
  • Photoresist
  • (Poly)Silicon
  • Aluminium
  • Chromium (ONLY RIE2!)
  • Other metals that covers less the 5% of the wafer area (ONLY RIE2!)
  • Photoresist
  • (Poly)Silicon
  • Aluminium
Etch rate

~70-90 nm/min (Thermal oxide)

  • Typically 40-120 nm/min can be increased or decreased by using other recipe parameters.
  • Typically 200-600 nm/min can be increased or decreased by using other recipe parameters.
Batch size
  • 1-25 wafers at a time
  • 1 wafer at a time
  • 1 wafer at a time
Size of substrate
  • 4" wafers
  • 4" wafers or smaller pieces
  • 6" or 4" depending on the setup (smaller pieces if you have a carrier wafer)
Allowed materials
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • Blue film
  • Gold (Au) and Nickel (Ni) (but only in BHF2 (KOH)!)
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resist
  • Aluminium
  • Chromium (ONLY RIE2!)
  • Other metals that covers less the 5% of the wafer area (ONLY RIE2!)
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resist
  • Aluminium