Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Silicon Nitride/Deposition of Silicon Nitride using PECVD: Difference between revisions

From LabAdviser
BGE (talk | contribs)
Line 2: Line 2:


==Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride==
==Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride==
 
===Recipes===
{| border="1" cellspacing="0" cellpadding="7"
|-
|Recipe name
|SiH4 flow [sccm]
|NH3 flow [sccm]
|N2 flow [sccm]
|Pressure [mTorr]
|Power [W]
|Description
|-
|1nitride
|
|
|
|
|
|
|-
|}


==Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride==
==Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride==

Revision as of 15:16, 28 November 2007

At the moment DANCHIP has 3 PECVDs that can deposite silicon nitride and silicon oxynitride. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and will be describes under III-V processing. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.

Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride

Recipes

Recipe name SiH4 flow [sccm] NH3 flow [sccm] N2 flow [sccm] Pressure [mTorr] Power [W] Description
1nitride

Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride

Recipes

Recipe name SiH4 flow [sccm] NH3 flow [sccm] N2 flow [sccm] Pressure [mTorr] Power [W] Description
MFSiNLS 30 30 1470 650 20HF 6s

20LF 2s

Low stress nitride - standard recipe
LFSiN 30 15 1470 550 60LF Compressive stress
HFSiN 30 42 1470 900 20HF Tensile stress

LF=Low Frequency HF=High Frequency MF=Mixed Frequency SiN=Silicon Nitride LS=Low Stress

Expected results

Recipe name Deposition rate [Å/min] RI Uniformity [%] Stress [MPa]
MFSiNLS ~117 ~1.99 ~-30
LFSiN ~550 ~1.96 ~3 ~-630
HFSiN ~130 ~1.97 ~2 ~460