Specific Process Knowledge/Thin film deposition/Deposition of Scandium Nitride/ScN Reactive Sputtering in Cluster Lesker PC3: Difference between revisions
| Line 502: | Line 502: | ||
==X-ray Photoelectron Spectroscopy== | ==X-ray Photoelectron Spectroscopy== | ||
X-ray | [[Specific Process Knowledge/Characterization/XPS|X-ray Photo Electron Spectroscopy (XPS)]] was employed to investigate the chemical composition of deposited scandium nitride (ScN) thin films using the [[Specific Process Knowledge/Characterization/XPS/K-Alpha|XPS K-Alpha]] instrument. The analysis was conducted in a 'depth profile' mode, where the film was incrementally etched, and the composition was measured layer by layer. Multiple scans were performed, including survey scans and scans for specific elements like O1s, N1s, Sc2p, Sc3s, and C1s, to gather comprehensive chemical information. | ||
Interpreting the stoichiometry of the ScN film is challenging due to the overlap between the N1s peak and the Sc2p peak. Additionally, while scandium has various interesting electronic states that can be measured and utilized in calculations (such as Sc3s), there is only one electronic state for nitrogen, N1s, which requires careful deconvolution from the Sc2p peak. | Interpreting the stoichiometry of the ScN film is challenging due to the overlap between the N1s peak and the Sc2p peak. Additionally, while scandium has various interesting electronic states that can be measured and utilized in calculations (such as Sc3s), there is only one electronic state for nitrogen, N1s, which requires careful deconvolution from the Sc2p peak. | ||
Revision as of 14:54, 9 November 2023
Feedback to this page: click here
This page is written by Evgeniy Shkondin @DTU Nanolab if nothing else is stated.
All images and photos on this page belongs to DTU Nanolab.
The fabrication and characterization described below were conducted in 2022 by Evgeniy Shkondin, DTU Nanolab.
This page presents the results of Scandium Nitride deposition using RF Reactive Sputtering in Sputter-System Metal-Nitride (PC3) commonly known as "Cluster Lesker". The deposition target is 4" Sc (0.25" Indium bonded to Cu plate). Source #1 was used. Materials (ScN) from this source can either be deposited with RF or p-DC sputtering although only RF mode has been tested so far.
The main focus of the study was the deposition rate, optical functions, and the general performance of deposition from a bigger 4” target. The scandium nitride sputtering from the target of this size allows achieving a higher deposition rate and service to many potential applications where several hundreds of nm are needed to be put uniformly on a wafer of 150 mm or similar. Additionally, the flexibility of this source (z-shift and tilting) allows tailoring the deposition output.
The most common application of scandium is its use as a dopant or addition to aluminum in the deposition of AlScN thin films. The presence of scandium enhances the preffered crystallographic orientation of aluminum nitride (AlN) and significantly improves the overall piezoelectric performance of the thin film. With the Cluster Lesker tool (PC3), scandium can be loaded into Source 1, while aluminum can be loaded into Source 2. Co-sputtering can then be performed from both sources, allowing for precise adjustment of individual powers, gas flows, and other parameters. This flexibility enables the tailoring of thin film stoichiometry and other properties to meet specific requirements.
4” magnetron in PC3 has more functionalities compared to the ordinary guns in cluster Lesker. It can(to some degree) moves in Z-direction. This will affect the deposition rate, uniformity and most likely play an important role in reactive sputtering. Besides that, it can be easily tilted if necessary. In this study, two z-high positions have been compared (lowest-“home” and highest –“extended”). The effect of power has also been evaluated.
Note! It seems that Scandium is prone to oxidation, better to keep the prepared samples in a inert environment.
RF Sputtering of Scandium Nitride in Sputter-System Metal-Nitride(PC3)
The RF ScN process recipe in a Sputter-System Metal-Nitride(PC3) is following:
* Recipe Name: MD PC3_Src1 - RF_Downstream with Reactive N2
- PC Gun Z-shift Position: Home (00.00 mm) and Extended (95.20 mm)
- Tilt: No (Target in horizontal plane)
- Deposition mode: Downstream
- Rotation speed: 10 rpm
- Pressure: 3 mTorr
- Power: 100-200 W (It is recommended to use 200W for getting high deposition rate and using "Extended" gun Z-shift position).
- Ar flow: 40 sccm
- N2 flow: 18 sccm
- Deposition time: 1000 s
- Deposition temperature: 400 °C
- Pre-sputtering time : 300s (better to give longer time to sputter away the native oxide, especially on a recently installed target)
Samples: 6" Si.
- The photography of Sc target mounted in 4” magnetron (PC3 Src1).
-
PC Gun Z-shift Position: Home (00.00 mm).
-
PC Gun Z-shift Position: Extended (95.20 mm).
Deposition Rate
- Scandium nitride thin film deposition rate (PC3 Src1) deposited at 400 °C.
-
Scandium nitride deposition rate as a function of power at two different PCZ-shift Gun positions.
| Scandium nitride deposition conditions | ||||||||||||||||||||||||||||||||||||||||||||||||||||
| ||||||||||||||||||||||||||||||||||||||||||||||||||||
X-ray Reflectivity (XRR)
- X-ray reflectivity scans of ScN thin films (PC3 Src1).
-
ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
-
ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
-
ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
- X-ray reflectivity scans of ScN thin films (PC3 Src1).
-
ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (00.00 mm).
-
ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (00.00 mm).
-
ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (00.00 mm).
Extracted values
| XRR results for ScN thin films deposited at 3 mTorr and different powers. PC Gun Z-shift Position: Extended (95.20 mm) | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| XRR results for ScN thin films deposited at 3 mTorr and different powers. PC Gun Z-shift Position: Home (00.00 mm) | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| Fitting parameters | |||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Sample | Moisture | ScNxOy | ScN | Sc-Si intermediate layer | Si substrate | Fitting parameters | |||||||||
| Delta | Beta | Delta | Beta | Delta | Beta | Delta | Beta | Delta | Beta | Intensity | Background | Fitting area () | R | ||
| PC Gun Z-shift Position: Extended (95.20 mm) 200W, 3mTorr, 500s | 1.9484E-6 | 4.5244E-8 | 8.9012E-6 | 2.0670E-7 | 1.3473E-5 | 1.2304E-6 | 9.3367E-6 | 2.1681E-7 | 7.5860E-6 | 1.7616E-7 | 1.30347E-000 | 3.58520E-007 | 0.4055 - 4.0000 | 0.01563 | 0.00513 |
| PC Gun Z-shift Position: Extended (95.20 mm) 150W, 3mTorr, 750s | 2.1902E-6 | 5.0859E-8 | 5.1589E-6 | 1.1980E-7 | 1.3736E-5 | 1.2545E-6 | 1.0416E-5 | 2.4187E-7 | 7.5860E-6 | 1.7616E-7 | 1.08491E-000 | 9.64995E-007 | 0.4055 - 4.0000 | 0.01452 | 0.00413 |
| PC Gun Z-shift Position: Extended (95.20 mm) 100W, 3mTorr, 1000s | 6.3024E-7 | 1.4635E-8 | 9.7505E-6 | 2.2642E-7 | 1.3484E-5 | 1.2314E-6 | 6.4131E-6 | 1.4892E-7 | 7.5860E-6 | 1.7616E-7 | 1.17155E-000 | 2.25376E-006 | 0.4055 - 4.0000 | 0.00744 | 0.00101 |
| PC Gun Z-shift Position: Home (00.00 mm) 200W, 3mTorr, 500s | 2.5771E-7 | 5.9844E-9 | 1.5175E-5 | 3.5239E-7 | 1.3596E-5 | 1.2417E-6 | 6.8990E-6 | 1.6020E-7 | 7.5860E-6 | 1.7616E-7 | 1.00181E-000 | 3.89203E-011 | 0.4055 - 4.0000 | 0.01830 | 0.00741 |
| PC Gun Z-shift Position: Home (00.00 mm) 150W, 3mTorr, 750s | 3.8018E-6 | 8.8284E-8 | 8.8171E-6 | 2.0475E-7 | 1.2333E-5 | 1.1264E-6 | 9.5589E-6 | 2.2197E-7 | 7.5860E-6 | 1.7616E-7 | 1.37654E-000 | 5.17162E-009 | 0.4055 - 4.0000 | 0.00825 | 0.00129 |
| PC Gun Z-shift Position: Home (00.00 mm) 100W, 3mTorr, 1000s | 5.2890E-6 | 1.2282E-7 | 7.1123E-6 | 1.6516E-7 | 1.2924E-5 | 1.1803E-6 | 1.0009E-5 | 2.3243E-7 | 7.5860E-6 | 1.7616E-7 | 1.19799E-000 | 1.15388E-006 | 0.4055 - 4.0000 | 0.00466 | 0.00039 |
X-ray Photoelectron Spectroscopy
X-ray Photo Electron Spectroscopy (XPS) was employed to investigate the chemical composition of deposited scandium nitride (ScN) thin films using the XPS K-Alpha instrument. The analysis was conducted in a 'depth profile' mode, where the film was incrementally etched, and the composition was measured layer by layer. Multiple scans were performed, including survey scans and scans for specific elements like O1s, N1s, Sc2p, Sc3s, and C1s, to gather comprehensive chemical information.
Interpreting the stoichiometry of the ScN film is challenging due to the overlap between the N1s peak and the Sc2p peak. Additionally, while scandium has various interesting electronic states that can be measured and utilized in calculations (such as Sc3s), there is only one electronic state for nitrogen, N1s, which requires careful deconvolution from the Sc2p peak.
The ScN sample used for XPS analysis was deposited at the PC Gun Z-shift Extended position (95.20mm) under the following conditions: 400°C, Ar/N 40/18 sccm, 200W power, 3mTorr pressure, and a deposition time of 1000 seconds.
- X-ray reflectivity scans of Sc thin films (PC3 Src1).
-
Sc thin film XRR. Power: 200W, Deposition time: 500s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
-
Sc thin film XRR. Power: 150W, Deposition time: 750s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
-
Sc thin film XRR. Power: 200W, Deposition time: 500s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
-
Sc thin film XRR. Power: 150W, Deposition time: 750s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
-
Sc thin film XRR. Power: 150W, Deposition time: 750s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
- X-ray reflectivity scans of Sc thin films (PC3 Src1).
-
Sc thin film XRR. Power: 200W, Deposition time: 500s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
-
Sc thin film XRR. Power: 200W, Deposition time: 750s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
-
Sc thin film XRR. Power: 200W, Deposition time: 750s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
-
Sc thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
- X-ray reflectivity scans of Sc thin films (PC3 Src1).
-
Sc thin film XRR. Power: 200W, Deposition time: 500s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
-
Sc thin film XRR. Power: 200W, Deposition time: 500s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
-
Sc thin film XRR. Power: 150W, Deposition time: 750s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
-
Sc thin film XRR. Power: 100W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
Scanning Electron microscopy
The images below present SEM images of the ScN layers from the top and tilted view.
- Scanning Electron Microscopy.
-
ScN layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Top view.
-
ScN layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Tilted view.
-
ScN layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Tilted view