The unique patterning setup (all-in-one) allowed complex in-situ deposition strategies. EBL routines for multi-layer and three-dimensional structuring were demonstrated. This opened up a wide range of possible directions to pursue in the future with this technique. | The unique patterning setup (all-in-one) allowed complex in-situ deposition strategies. EBL routines for multi-layer and three-dimensional structuring were demonstrated. This opened up a wide range of possible directions to pursue in the future with this technique. | ||
==Etching== | ==Etching== | ||
As other organic lithographic resists, OIR patterns are able to withstand the chemical and physical action of reactive species protecting the underlying material, while the surrounding areas are gradually removed. | |||
We initially demonstrated this process to create silicon nanostructures on the sample surface. The silicon etch consisted of a two-phase Bosch process iterating an isotropic etching step based on SF6 plasma and a sidewall passivation step. For nonane ice patterns, selectivity over silicon was 1:6, which is the same value obtained with AR-N 7520. | |||
We then used similar samples made from silicon wafers with a layer of silicon oxide thermally grown on its surface. We structured the SiO2 layer using patterned OIR features as mask in one of our cleanroom's oxide RIE tools for photoresist. The recipe consisted in a single step, a continuous flow etch based on C4F8. The oxide etch process resulted in rougher and more shallow lines, due to limited etch resistance. The selectivity for the SiO2 RIE was 1:1.6; the corresponding value for AR-N 7520 was not measured since the profiles were not satisfying, requiring further optimization. | |||
==Diamond Nanofabrication== | ==Diamond Nanofabrication== | ||
Revision as of 14:06, 15 June 2018
Feedback to this page: click here
Electron-Beam Lithography on Organic Ice Resists
Overview
Resist thickness ranged between 7 nm up to 2 µm, with best results obtained for films around 20-200 nm, deposited in 5-10 min.
Critical dose was dependent on acceleration voltage and OIR, with the lowest observed at 3 mC/cm2 for nonane OIR exposed at 5 keV. The resolution achievable with the SEM LEO was limited to above 50 nm due to vibrations in the column and stage; still, an alternative cryo-ETEM setup at DTU Cen was developed from the project confirming sub-10 nm resolution.
A variety of sample geometries was tested in the SEM tool, as small as 2 mm in size and as thin as 5 nm membranes. Their patterning could be accommodated at no added effort, as with IL.
Organic Ice Resists
Contrast Curve
Multi-layers
The unique patterning setup (all-in-one) allowed complex in-situ deposition strategies. EBL routines for multi-layer and three-dimensional structuring were demonstrated. This opened up a wide range of possible directions to pursue in the future with this technique.
Etching
As other organic lithographic resists, OIR patterns are able to withstand the chemical and physical action of reactive species protecting the underlying material, while the surrounding areas are gradually removed.
We initially demonstrated this process to create silicon nanostructures on the sample surface. The silicon etch consisted of a two-phase Bosch process iterating an isotropic etching step based on SF6 plasma and a sidewall passivation step. For nonane ice patterns, selectivity over silicon was 1:6, which is the same value obtained with AR-N 7520.
We then used similar samples made from silicon wafers with a layer of silicon oxide thermally grown on its surface. We structured the SiO2 layer using patterned OIR features as mask in one of our cleanroom's oxide RIE tools for photoresist. The recipe consisted in a single step, a continuous flow etch based on C4F8. The oxide etch process resulted in rougher and more shallow lines, due to limited etch resistance. The selectivity for the SiO2 RIE was 1:1.6; the corresponding value for AR-N 7520 was not measured since the profiles were not satisfying, requiring further optimization.